# X17CrNi16-2 (1.4057 / AISI 431) Open-Die Forgings

**Manufacturer:** Jiangyin Jiangnan Metal Co., Ltd., open-die forging factory
**Address:** No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
**Tel:** +86-189-2135-9659 | **Email:** sales@steelforgepieces.com
**Source page:** https://www.steelforgepieces.com/Stainless-Steel/X17CrNi16-2.html
**Last reviewed:** 9 October 2026 | **Material standard:** EN 10088-3 / EN 10250-4

## Summary

X17CrNi16-2 (EN material number 1.4057, AISI 431, UNS S43100) is a martensitic chromium-nickel stainless steel with 0.12-0.22 % C, 15.0-17.0 % Cr and 1.5-2.5 % Ni. The nickel addition gives it higher toughness and better corrosion resistance than the plain 12 % chromium martensitic grades. It is normally used quenched and tempered to +QT800 (Rm 800-950 MPa) or +QT900 (Rm 900-1050 MPa), is ferromagnetic, machines well, forges well, and is usable to about 400 °C.

Jiangyin Jiangnan Metal Co., Ltd. supplies X17CrNi16-2 as forged round, square, flat and hex bars, forged and seamless rolled rings, discs and blocks, hollow bars and sleeves, and machined shafts, spindles, piston rods and valve components.

| Key figure | Value |
| --- | --- |
| EN designation | 1.4057 / X17CrNi16-2 |
| US equivalent | AISI 431 / UNS S43100 |
| Density | 7.70 kg/dm³ |
| Tensile strength, +QT800 | 800-950 MPa, Rp0.2 min 600 MPa |
| Forging range | 1180-950 °C, slow cooling |
| Magnetic | Yes, ferromagnetic |

## 1. Grade description

X17CrNi16-2 is the EN designation for a hardenable corrosion-resisting chromium-nickel steel that transforms to martensite on quenching. It is specified where the 12 % chromium martensitic grades do not give enough corrosion resistance, or where their toughness falls short. The 15-17 % chromium content raises corrosion resistance, and the 1.5-2.5 % nickel addition keeps the structure fully martensitic rather than part ferritic at that chromium level, which is what preserves impact toughness after heat treatment.

The grade is covered by EN 10088-1 (list of stainless steels), EN 10088-3 (semi-finished products, bars, rods, sections and bright products), EN 10088-5 (construction purposes), EN 10272 (stainless steel bars for pressure purposes) and EN 10250-4 (open steel die forgings for general engineering purposes: stainless steels). Use within the scope of the European Pressure Equipment Directive is possible subject to prior agreement.

Corrosion resistance, mechanical properties, forgeability and machinability are all rated good; weldability is rated poor, and the service ceiling is around 400 °C. The pitting resistance equivalent is 17.5 to 21.26, placing it among the moderately corrosion-resistant steels. It does not replace 316L or a duplex grade in chloride service.

## 2. Chemical composition (% by mass)

| Standard and grade | C | Si | Mn | P | S | Cr | Ni |
| --- | --- | --- | --- | --- | --- | --- | --- |
| **EN X17CrNi16-2 (1.4057)** | 0.12-0.22 | max 1.00 | max 1.50 | max 0.040 | max 0.030 | 15.0-17.0 | 1.5-2.5 |
| ASTM AISI 431 / UNS S43100 | max 0.20 | max 1.00 | max 1.00 | max 0.040 | max 0.030 | 15.0-17.0 | 1.25-2.5 |
| LW 1.4044 | 0.12-0.20 | max 1.00 | max 1.00 | max 0.035 | max 0.025 | 15.0-18.0 | 2.0-3.0 |
| EN X19CrNi17-2 | 0.14-0.23 | max 1.00 | max 1.00 | max 0.040 | max 0.015 | 15.5-17.5 | 1.5-2.5 |
| AFNOR Z15CN16-02 | 0.15-0.20 | max 1.00 | max 1.00 | max 0.040 | max 0.025 | 15.5-17.0 | 1.5-2.5 |
| GOST 14Ch17N2 | 0.11-0.17 | max 0.80 | max 0.80 | max 0.030 | max 0.025 | 16.0-18.0 | 1.5-2.5 |
| GOST 20Ch17N2 | 0.17-0.25 | max 0.80 | max 0.80 | max 0.035 | max 0.025 | 16.0-18.0 | 1.5-2.5 |
| PN H17N2A | 0.11-0.17 | max 0.80 | max 0.80 | max 0.035 | max 0.020 | 16.0-18.0 | 1.5-2.5 |

The EN and ASTM windows are not identical. AISI 431 allows nickel down to 1.25 % and limits manganese to 1.00 %, while X17CrNi16-2 permits up to 1.50 % Mn and sets a carbon floor of 0.12 %. For dual certification we restrict the melt analysis to the overlap of both windows; state this at the enquiry stage.

## 3. Equivalents and other designations

| System or country | Designation |
| --- | --- |
| EN and Werkstoffnummer (Europe) | X17CrNi16-2, X 17 CrNi 16-2, 1.4057, DIN 17440 1.4057 |
| ASTM / AISI / UNS (USA) | AISI 431, UNS S43100, Aeralloy 431-C |
| Aerospace | AMS 5628, WL 1.4044, AIR 9160 Z15CN17-03, ASNA 3126 / 3138 / 3299 |
| JIS (Japan) | SUS 431 |
| BS (United Kingdom) | 431S29, 321S31, S80 |
| AFNOR (France) | Z15CN16-02, Z15CN17-03, Z15CN17.03 |
| SIS (Sweden) | 2321 |
| GOST (Russia and CIS) | 14Ch17N2 (14172), 20Ch17N2 (20172), 1Ch17N2 |
| PN (Poland) | H17N2, H17N2A, 2H17N2 |
| Close variants | 1.4044, X19CrNi17-2, X20CrNi17-2, X22CrNi17, X16CrNi16, X14CrNi172 |

Equivalence is approximate. Cross-reference tables match grades by chemistry family, not by guaranteed properties, test regime or delivery condition. Order to the exact standard named on the drawing.

## 4. Mechanical properties

Room temperature, longitudinal, per EN 10088-3 together with typical mill values. The number after QT is the minimum tensile strength in N/mm².

| Condition | Rp0.2 (MPa) | Rm (MPa) | A5 (%) | ISO-V at 20 °C (J) | Hardness HB |
| --- | --- | --- | --- | --- | --- |
| +A annealed | approx. 275 | max 950 | - | - | max 295 |
| **+QT800** specified | min 600 | 800-950 | min 14 | min 25 | - |
| +QT800 typical | 620 | 820 | 20 | - | approx. 251-299 |
| **+QT900** specified | min 700 | 900-1050 | min 12 | min 25 | - |
| +QT900 typical | 710 | 920 | 16 | - | - |

Elongation and impact values are section sensitive. In +QT800, EN 10088-3 requires A ≥ 14 % and KV ≥ 25 J up to 60 mm, relaxing to A ≥ 12 % and KV ≥ 20 J above 60 mm; above roughly 160 mm the properties are agreed between purchaser and supplier. For heavy open-die forgings we quote guaranteed values against the actual ruling section and test location.

In the annealed condition the yield strength is only about 275 MPa, so the grade is normally machined or cold formed soft and hardened afterwards. Straightening of profiles up to 35 mm can raise hardness by up to about 60 HB and tensile strength by up to about 150 N/mm² above the annealed figures.

### Minimum 0.2 % proof stress at temperature (MPa, EN 10088-3)

| Condition | 100 °C | 150 °C | 200 °C | 250 °C | 300 °C | 350 °C | 400 °C |
| --- | --- | --- | --- | --- | --- | --- | --- |
| +QT800 | 515 | 495 | 475 | 460 | 440 | 405 | 355 |
| +QT900 | 565 | 525 | 505 | 490 | 470 | 430 | 375 |

## 5. Physical properties

| Property | Value |
| --- | --- |
| Density | 7.70 kg/dm³ (7.7 g/cm³) |
| Electrical resistivity at 20 °C | 0.70 Ω·mm²/m |
| Thermal conductivity at 20 °C | 25 W/(m·K) |
| Specific heat capacity at 20 °C | 460 J/(kg·K) |
| Coefficient of thermal expansion | 10.0 × 10⁻⁶ K⁻¹ (20-100 °C); 10.5 × 10⁻⁶ K⁻¹ (20-200, 20-300, 20-400 °C) |
| Magnetisability | Yes, ferromagnetic in all conditions |
| Maximum service temperature | approx. 400 °C |
| PRE, pitting resistance equivalent | 17.5 to 21.26 |

Because the grade is ferromagnetic, forgings can be inspected by magnetic particle testing, where austenitic stainless steels require dye penetrant instead. MT, PT, UT and hardness survey reports are available on request.

## 6. Forging and heat treatment

**Forging.** Heat gradually to about 850 °C, then more rapidly to 1150-1180 °C. Forge between 1180 °C and 950 °C and cool slowly in a furnace or buried in dry ash. The steel is air hardening, so air cooling a heavy section straight from forging risks quench cracking.

**Soft annealing (+A).** Hold between 680 °C and 800 °C, then cool slowly in the furnace or in air. This is the condition for rough machining.

**Hardening and tempering.** Austenitise between 950 °C and 1060 °C and quench in oil or air. For +QT800, temper at 750-800 °C followed by a second temper at 650-700 °C. For +QT900, temper at 600-650 °C. Where the nickel content of the heat sits at the low end of the specification, a single temper between 620 °C and 720 °C is sufficient for +QT800.

**475 °C embrittlement.** The grade is susceptible to embrittlement in the 420-520 °C band. Exposure to this range has to be limited during fabrication and in service, which is the main reason the service ceiling is around 400 °C.

## 7. Machining, welding and corrosion behaviour

**Machinability.** Rated good and governed largely by hardness; the steel cuts much like a carbon steel of equivalent hardness and is easier to machine than conventional austenitic stainless steels. Starting point with coated carbide tooling on solution annealed material at Rm 700-800 N/mm²: 100 m/min at 6 mm depth of cut and 0.5 mm/rev, 130 m/min at 3 mm and 0.4 mm/rev, 165 m/min at 1 mm and 0.2 mm/rev.

**Welding.** Weldability is rated poor. With a matching filler, preheat to 100-300 °C and temper as soon as possible after welding; re-heat-treat the whole component for optimum properties. Where weld metal strength is not critical, an austenitic filler (4430 or 4370 type) can be used without preheat. Avoid nitrogen and carbon bearing shielding gases, and remove spatter and heat tint to restore corrosion resistance. Cold forming and cold heading are not common practice on this grade.

**Corrosion resistance.** Good for a martensitic steel and best in the hardened and tempered condition with a smooth polished surface. The grade resists nitric acid and other strongly oxidising acids, phosphoric acid, dilute formic and acetic acids, most nitrates, and sea water in intermittent service. Its limitation is intergranular corrosion caused by chromium carbide precipitation; welded or improperly tempered parts need post-weld heat treatment.

## 8. Typical applications

Mechanical engineering, chemical and petrochemical plant, automotive, marine and shipbuilding, aerospace, and the paper, nitrogen and food industries. Typical parts: heavily loaded pump parts and pump casings, valve bodies, valve stems and internals, drive and propeller shafts, sleeves and bushings, spindles, piston rods, fittings, stirrers and mixing blades, gears, actuators, bearings, hydraulic rams, crane pins, bolts, nuts and other fasteners. The H17N2A variant is a special aerospace grade used for aircraft parts.

## 9. Forgings we manufacture in this grade

Forged round, square, rectangular, flat and hex bars. Forged rings and radial-axial seamless rolled rings, including flange rings, gear blanks and bearing rings. Forged discs, disks, blocks, slabs and heavy plate. Forged hollow bars, sleeves, bushes and bushings, pipes and tubes, barrels, casings, shells, cylinders, hubs and housings. Shafting, stepped shafts, spindles, piston rods and stems. Pump parts, valve parts, valve bodies and bonnets, and near-net-shape open-die and die forgings to drawing.

Delivery conditions: as forged, +A annealed, +QT800 and +QT900. Standard documentation is an EN 10204 3.1 inspection certificate covering chemical analysis, mechanical test results and heat treatment records. Third-party inspection and witness testing can be arranged.

## 10. Frequently asked questions

**What is X17CrNi16-2 steel?**
X17CrNi16-2 (EN material number 1.4057) is a martensitic chromium-nickel stainless steel containing 0.12-0.22 % carbon, 15.0-17.0 % chromium and 1.5-2.5 % nickel. It is listed in EN 10088-1, EN 10088-3, EN 10088-5, EN 10272 and EN 10250-4, and is normally supplied quenched and tempered to +QT800 or +QT900. It is ferromagnetic and usable to about 400 °C.

**What is X17CrNi16-2 equivalent to?**
EN 1.4057, AISI 431, UNS S43100, SUS 431 (Japan), BS 431S29 and 321S31 (UK), Z15CN16-02 and Z15CN17-03 (France), SIS 2321 (Sweden), AMS 5628 (aerospace), WL 1.4044 and X19CrNi17-2, GOST 14Ch17N2 and 20Ch17N2, and the Polish grades H17N2, H17N2A and 2H17N2.

**What is the difference between +QT800 and +QT900?**
The figure after QT is the minimum tensile strength in N/mm². +QT800 is tempered at 750-800 °C with a second temper at 650-700 °C and gives Rm 800-950 MPa, Rp0.2 ≥ 600 MPa and A ≥ 14 %. +QT900 is tempered at 600-650 °C and gives Rm 900-1050 MPa, Rp0.2 ≥ 700 MPa and A ≥ 12 %.

**Can X17CrNi16-2 be welded?**
Yes, but weldability is rated poor. With a matching filler, preheat to 100-300 °C and temper immediately after welding; re-heat-treat the whole part for full properties. Austenitic fillers avoid the preheat where weld strength is not critical.

**At what temperature is X17CrNi16-2 forged?**
Heat gradually to about 850 °C, then more rapidly to 1150-1180 °C. Forge between 1180 °C and 950 °C and cool slowly in a furnace or dry ash. Avoid prolonged exposure to 420-520 °C because of 475 °C embrittlement.

**Is X17CrNi16-2 magnetic?**
Yes, ferromagnetic in every delivery condition, so magnetic particle inspection can be used on finished forgings.

**Who supplies X17CrNi16-2 open-die forgings?**
Jiangyin Jiangnan Metal Co., Ltd., an open-die forging factory at No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China, manufactures X17CrNi16-2 (1.4057 / AISI 431) forged bars, rings, discs, hollow bars, shafts and pump and valve forgings. Contact +86-189-2135-9659 or sales@steelforgepieces.com.

## References

- EN 10088-1, EN 10088-3, EN 10088-5, EN 10272 and EN 10250-4 standard listings for 1.4057 — steelnumber.com
- Deutsche Edelstahlwerke / Swiss Steel Group data sheet 1.4057 (physical properties, heat treatment, forging, welding, machining, PRE)
- Comparative composition, delivery conditions and equivalents for X17CrNi16-2 / AISI 431 — Virgamet
- Masteel UK and AZoM, Applications of Martensitic Stainless Steel 1.4057 QT800

Data compiled from the published standards and mill data sheets listed above, for general guidance. Guaranteed values for a specific order are those stated on the material certificate supplied with the forging.

## Contact

Jiangyin Jiangnan Metal Co., Ltd. — Open-Die Forging Factory
No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
Tel +86-189-2135-9659 | Email sales@steelforgepieces.com