# X15CrNiSi25-20 Forgings: 1.4841 / AISI 314 Rings, Flanges, Shafts and Bars

**Supplier:** Jiangyin Jiangnan Metal Co., Ltd. (open-die forging factory)
**Address:** No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
**Tel:** +86-189-2135-9659 | **Email:** sales@steelforgepieces.com
**Page:** https://www.steelforgepieces.com/Stainless-Steel/X15CrNiSi25-20.html
**Last reviewed:** 9 October 2026

## Summary

X15CrNiSi25-20, material number 1.4841, AISI 314, UNS S31400, is a heat-resistant
austenitic stainless steel containing 24-26 % chromium, 19-22 % nickel and
1.5-2.5 % silicon. The high silicon content gives scaling resistance in air up to
about 1150 C, which is why the grade is specified for furnace internals, burner
components, recuperators and petrochemical hot-gas hardware. Jiangyin Jiangnan
Metal Co., Ltd., an open-die forging factory in Jiangyin, Jiangsu, China, forges
this grade into rings, seamless rolled rings, flanges, shafts, discs, sleeves,
bushings and bars to customer drawing, with EN 10204 3.1 or 3.2 certification.

| Key data | Value |
| --- | --- |
| Material number | 1.4841 |
| EN 10095 designation | X15CrNiSi25-21 |
| SEW 470 / DIN designation | X15CrNiSi25-20 |
| AISI / UNS | 314 / S31400 |
| Structure | Austenitic, not magnetisable |
| Scaling resistance in air | about 1150 C |
| Tensile strength Rm | 550-750 N/mm2 |
| Density | 7.9 g/cm3 |

## Designations and international equivalents

X15CrNiSi25-20 and X15CrNiSi25-21 both refer to material number 1.4841. The 25-20
form comes from the older SEW 470 and DIN practice. The 25-21 form is the
designation in the current EN 10095 standard for heat-resisting steels. The
practical difference is a slightly wider nickel band in EN 10095.

| Standard or region | Designation | Remark |
| --- | --- | --- |
| EN 10095 (Europe) | X15CrNiSi25-21, 1.4841 | Current designation |
| SEW 470 / DIN | X15CrNiSi25-20, 1.4841 | Former designation, Ni 19.0-21.0 % |
| AISI / UNS (USA) | AISI 314, UNS S31400 | Closest equivalent |
| AISI / UNS (related) | AISI 310, UNS S31000 | Lower Si, lower scaling resistance |
| BS (UK) | 314S25 | |
| AFNOR (France) | Z15CNS25-20 | C max 0.15 % |
| UNE (Spain) | F-3310 | |
| GOST (Russia) | 20Kh25N20S2 | Si 2.0-3.0 % |
| PN (Poland) | H25N20S2 | Si 2.0-3.0 % |
| JIS (Japan) | SUH 310 | Related heat-resisting grade |
| GB (China) | 16Cr25Ni20Si2, 2Cr25Ni20 | Related heat-resisting grade |
| DIN tool-steel listing | X16CrNiSi25-20, 1.2782 | Si 1.8-2.3 % |

Cross-references are for guidance. Chemistry bands differ slightly between
standards, so confirm the specification to be certified before the order is
released.

## Chemical composition (weight %, EN 10095 / SEW 470)

| C | Si | Mn | P | S | Cr | Ni | N | Mo | Fe |
| --- | --- | --- | --- | --- | --- | --- | --- | --- | --- |
| max 0.20 | 1.50-2.50 | max 2.00 | max 0.045 | max 0.015 | 24.00-26.00 | 19.00-22.00 | max 0.11 | not specified | Balance |

SEW 470 limits nickel to 19.0-21.0 %. Older DIN sources give S max 0.030 %.
Molybdenum, V, W, Ti, Cu, Al, Nb and B are not alloying elements in this grade.

## Mechanical properties (solution annealed, 20 C, sections up to about 160 mm)

| Property | Value |
| --- | --- |
| 0.2 % proof stress Rp0.2 | min 230 N/mm2 |
| 1.0 % proof stress Rp1.0 | min 270 N/mm2 |
| Tensile strength Rm | 550-750 N/mm2 |
| Elongation after fracture A | min 30 %, min 28 % transverse |
| Hardness | max 223 HB |
| Modulus of elasticity | 196-210 kN/mm2 |
| Magnetisable | No |

### Creep rupture strength Rz and 1 % creep limit R1 (MPa)

| Temp. C | Rz 1000 h | Rz 10 000 h | Rz 100 000 h | R1 1000 h | R1 10 000 h |
| --- | --- | --- | --- | --- | --- |
| 600 | 170 | 130 | 80 | 105 | 95 |
| 700 | 90 | 40 | 18 | 50 | 35 |
| 800 | 40 | 20 | 7 | 23 | 10 |
| 900 | 20 | 10 | 3 | 10 | 4 |
| 1000 | 5 | | | 3 | |

Long-term high-temperature figures are published typical values for design
guidance, not guaranteed acceptance values.

## Physical properties

| Property | Value |
| --- | --- |
| Density | 7.9 g/cm3 |
| Specific heat capacity | 500 J/(kg K) |
| Thermal conductivity | 15 W/(m K) at 20 C, 19 W/(m K) at 500 C |
| Electrical resistivity | 0.90 ohm mm2/m at 20 C, 1.25 at 1000 C |

Mean coefficient of linear thermal expansion, 10-6 / K:
20-200 C: 15.5 | 20-400 C: 17.0 | 20-600 C: 17.5 | 20-800 C: 18.0 |
20-1000 C: 19.0 | 20-1200 C: 19.5

## Forging, heat treatment and fabrication

**Forging.** Hot forming runs between 1150 C and 800 C, followed by cooling in
air. The grade work-hardens quickly, so passes and reheats are planned to keep
the finishing temperature above 800 C, after which the forging is solution
annealed.

**Heat treatment.** Supplied solution annealed at 1050-1150 C followed by rapid
cooling, in water or in air for thin sections. Being austenitic, the grade cannot
be hardened by quenching or by ageing. Strength is raised only by cold work.
Stress relieving after machining is done at about 650 C for 1 to 2 hours with air
cooling.

**Machining.** Comparable with type 304. Chips are stringy and the material
work-hardens fast, so use positive rake, rigid setups, chip breakers and plenty
of coolant, and keep the tool cutting.

**Welding.** Weldable by the usual fusion and resistance processes.
Oxyacetylene welding is not recommended. Common fillers are AWS E or ER 309 and
309L, or matching 1.4842 type consumables.

**Service limits.** Scaling resistant in air to about 1150 C, with continuous
service normally planned at 1050-1100 C and some datasheets setting 1000 C under
mechanical load. Sensitive to SO2 and H2S above 650 C and to carburising gases
above about 900 C. Tendency to sigma phase embrittlement on long exposure between
600 C and 850 C. Creep resistant to roughly 690 C.

## Forged products available in X15CrNiSi25-20

- Rings and seamless rolled rings, radial-axial rolled rings, retaining rings, valve seat rings
- Forged flanges, blind flanges, weld-neck and custom-profile flange blanks
- Round, square and flat bars, shafts, spindles, eccentric shafts, stepped shafts
- Forged discs and disks, blanks for gears, wheels, covers and closures
- Sleeves, hollow bars, bushings, cylinders, liners
- Forged tube blanks, tube sheets, nozzles, manifolds, pipe sections
- Valve bodies, valve blocks, valve stems, bonnets, seat rings
- Custom open-die forgings: blocks, cubes, step forgings, near-net shapes

Dimensions depend on part geometry and ingot availability. Send the drawing, or
OD x ID x height and weight, for confirmation of feasibility, price and lead time
within 24 hours.

## Typical applications

- Industrial furnaces and thermal processing: annealing covers and boxes, muffles and retorts, burner grids, furnace doors, fans, walking beams, recuperators
- Petrochemical and refining: catalytic recovery systems, FCC internals, flares, tube hangers, hot-gas piping components
- Cement, lime and sintering plants: burners and burner shields, preheater parts, feeding and discharging systems, wind boxes
- Power and combustion: fluidised-bed furnace parts, coal combustor grids, superheater components, steam boiler fittings, thermocouple sheath tubes
- Steel and ore processing: smelter and steel melting equipment, continuous casting hardware
- Glass and chemical process: gas pyrolysis and methane conversion equipment, glass-blowing pipe ends, hydrogenation components, columns and towers

1.4841 is a high-silicon heat-resisting grade for elevated temperature service.
For cryogenic duty, ask about A182-F321 or another austenitic grade.

## Melting, testing and certification

- Melting routes: EAF plus VOD, or ESR remelt where improved cleanliness is specified
- Ultrasonic inspection to EN 10228-3, SEP 1921 or ASTM A388; PT and MT on request
- Tensile, hardness, impact and elevated-temperature testing from prolongations or test rings
- Ladle and product chemical analysis by spectrometry
- Inspection certificate EN 10204 3.1, or 3.2 witnessed by TUV, SGS, BV or Lloyd's
- Supply condition: solution annealed, rough turned or proof machined, or finish machined to drawing

## Frequently asked questions

**What is X15CrNiSi25-20 steel?**
A heat-resistant austenitic chromium-nickel-silicon stainless steel, material
number 1.4841, with 24-26 % Cr, 19-22 % Ni and 1.5-2.5 % Si. Silicon promotes a
protective oxide scale, giving scaling resistance in air up to about 1150 C.

**Is X15CrNiSi25-20 the same as X15CrNiSi25-21?**
In practice yes, both are 1.4841. X15CrNiSi25-20 is the older SEW 470 and DIN
designation with Ni 19.0-21.0 %; X15CrNiSi25-21 is the EN 10095 designation with
Ni 19.0-22.0 %.

**What is the AISI equivalent of 1.4841?**
AISI 314, UNS S31400. The grade is also cross-referenced to AISI 310 and 310S,
UNS S31000, but 310 carries less silicon and has lower scaling resistance.

**What is the maximum service temperature?**
Scaling resistance in air is quoted at about 1150 C. Continuous service is
generally planned at 1050-1100 C, with 1000 C used as the limit under mechanical
load in some mill datasheets.

**Can the grade be hardened by heat treatment?**
No. It is fully austenitic and cannot be hardened by quenching or ageing. It is
delivered solution annealed from 1050-1150 C with rapid cooling.

**Is X15CrNiSi25-20 weldable?**
Yes, by normal fusion and resistance methods. Oxyacetylene welding is not
recommended. Usual fillers are AWS E or ER 309 and 309L, or matching 1.4842 type
consumables. Avoid long exposure of the weldment to 600-850 C.

**How do I get a quotation?**
Email the drawing or dimensions, standard, condition and certificate level to
sales@steelforgepieces.com, or call +86-189-2135-9659. Reply within 24 hours with
price, forged weight and lead time.

## Contact

Jiangyin Jiangnan Metal Co., Ltd.
No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
Tel +86-189-2135-9659 | Email sales@steelforgepieces.com
Open-die forgings, seamless rolled rings, forged flanges, shafts, discs, sleeves
and bars in stainless, heat-resistant, alloy, tool and nickel-base materials.

Technical data compiled from EN 10095, SEW 470 and published mill datasheets for
material 1.4841. Given for guidance; it does not replace the agreed order
specification.