title: "X10CrNi18-8 (EN 1.4310 / AISI 301) Open-Die Forgings"
description: "EN 10088 composition, mechanical and physical data, forging and annealing temperatures and corrosion limits for X10CrNi18-8 stainless steel forgings."
canonical: "https://www.steelforgepieces.com/Stainless-Steel/X10CrNi18-8.html"
grade: "X10CrNi18-8"
en_number: "1.4310"
uns: "S30100"
aisi: "301"
structure: "Austenitic, metastable"
supplier: "Jiangyin Jiangnan Metal Co., Ltd."
supplier_location: "Zhouzhuang Town, Jiangyin City, Jiangsu Province, China"
supplier_phone: "+86 189 2135 9659"
supplier_email: "sales@steelforgepieces.com"
updated: "2026-10-09"
---

# X10CrNi18-8 (EN 1.4310 / AISI 301) Open-Die Forgings

**X10CrNi18-8 is an austenitic chromium-nickel stainless steel carrying EN material number 1.4310**, covered by EN 10088-1, EN 10088-2, EN 10088-3, EN 10151, EN 10263-5 and EN ISO 6931-1. It contains 0.05 to 0.15 % carbon, 16.0 to 19.0 % chromium and 6.0 to 9.5 % nickel. The nickel content is deliberately held low, which leaves the austenite metastable: the steel work hardens very quickly under cold deformation, and part of the structure turns to martensite as it does so. That single property explains almost everything else about the grade, from its use as a spring steel to its awkward machining behaviour.

Jiangyin Jiangnan Metal Co., Ltd. melts this grade rather than buying billet. Stainless heats run through the electric arc furnace, the ladle furnace and vacuum oxygen decarburisation, then go to the presses and the ring mill without leaving the site, so the certificate traces back to a melt number instead of stopping at a purchased bar.

| Key data | Value |
|---|---|
| EN name | X10CrNi18-8 |
| EN number | 1.4310 |
| US / UNS | AISI 301, UNS S30100 |
| Structure | Austenitic, metastable |
| Density | 7.9 kg/dm³ |
| Rm, annealed | 500 to 700 MPa |
| Rp0.2, annealed | 195 MPa minimum |
| Hardness | 230 HB maximum |
| PREN | 16.0 to 23.4 |
| Forging range | 1150–1200 °C down to 900 °C |
| Solution anneal | 1000 to 1100 °C, rapid cool |
| Maximum spring service temperature | 300 °C |

## 1. Chemical composition

Composition limits follow EN 10088. Elements outside this list are not added deliberately, except as needed to finish the cast.

Table 1 — X10CrNi18-8 / 1.4310 chemical composition, mass %, to EN 10088.

| C | Si | Mn | P | S | Cr | Ni | Mo | N |
|---|---|---|---|---|---|---|---|---|
| 0.05–0.15 | max 2.00 | max 2.00 | max 0.045 | max 0.015 | 16.0–19.0 | 6.0–9.5 | max 0.80 | max 0.11 |

**Molybdenum is not an alloying addition in this grade.** The 0.80 % figure is a residual ceiling only, and a good deal of material published about 1.4310 gets this wrong. Where molybdenum is needed for chloride pitting resistance, specify 904L, A182 F44 or a duplex grade such as A182 F51.

The calculated pitting resistance equivalent runs from 16.0 to 23.4, depending on where chromium, molybdenum and nitrogen fall inside the band.

## 2. Equivalent grades

The EN band is wider than AISI 301 on both chromium and nickel, so state the governing standard on the order where the distinction matters to the end user.

Table 2 — X10CrNi18-8 (1.4310) international equivalents.

| Region and standard | Designation |
|---|---|
| EU, EN 10088-3 | X10CrNi18-8 / 1.4310 |
| USA, AISI and UNS | AISI 301 (UNS S30100), AISI 302 (UNS S30200) |
| USA, AMS | AMS 5516 |
| Germany, DIN 17440, withdrawn | X12CrNi17-7 |
| Japan, JIS | SUS 301, SUS 302 |
| United Kingdom, BS | 301S21, 302S26 |
| France, AFNOR | Z11CN17-08, Z12CN18-09, Z12CN17-07 |
| Sweden, SS | 2331 |
| Russia, GOST | 12Kh18N9 |
| Poland, PN | 1H18N9 |
| Spain, UNE | F-3507, X10CrNi18-9 |
| Czech Republic | 17241, 17242 |
| International, ISO | X9CrNi18-8 |

## 3. Mechanical properties

Values apply to the solution annealed condition at room temperature, tested longitudinally.

Table 3 — Mechanical properties, solution annealed.

| Property | Symbol | Value |
|---|---|---|
| 0.2 % proof strength | Rp0.2 | 195 MPa minimum |
| 1.0 % proof strength | Rp1.0 | 230 MPa minimum |
| Tensile strength | Rm | 500 to 700 MPa |
| Elongation at fracture | A | 40 % minimum |
| Brinell hardness | HB | 230 maximum |
| Modulus of elasticity, 20 °C | E | 200 GPa |

Table 4 — Elevated temperature proof strength, solution annealed.

| Temperature | 100 °C | 150 °C | 200 °C | 250 °C | 300 °C |
|---|---|---|---|---|---|
| Rp0.2, MPa | 210 | 200 | 190 | 185 | 180 |
| Rp1.0, MPa | 230 | 215 | 205 | 200 | 195 |

Cold rolling and drawing lift the strength far above the annealed level because the metastable austenite converts to deformation martensite as it deforms. EN 10151 defines the conditions below for strip and spring material. They are listed for reference: forgings are supplied solution annealed, not cold worked.

Table 5 — Cold-worked conditions to EN 10151.

| Condition | Tensile strength Rm | Elongation A |
|---|---|---|
| +C850 | 850 to 1000 MPa | 25 % min |
| +C1000 | 1000 to 1150 MPa | 20 % min |
| +C1150 | 1150 to 1300 MPa | 15 % min |
| +C1300 | 1300 to 1500 MPa | 10 % min |
| +C1500 | 1500 to 1700 MPa | 5 % min |
| +C1700 | 1700 to 1900 MPa | 2 % min |
| +C1900 | 1900 to 2200 MPa | 1 % min |

**Heavy sections.** Above about 160 mm diameter the values in Table 3 are not automatically guaranteed through thickness. Test location, sampling direction and acceptance values are agreed with the purchaser before forging starts, not after the part is on the test bench.

## 4. Physical properties

Table 6 — Physical properties of X10CrNi18-8 (1.4310).

| Property | Value |
|---|---|
| Density at 20 °C | 7.9 kg/dm³ |
| Electrical resistivity at 20 °C | 0.73 Ω·mm²/m |
| Thermal conductivity at 20 °C | 15 W/(m·K) |
| Specific heat capacity at 20 °C | 500 J/(kg·K) |
| Linear expansion, 20 to 100 °C | 16 × 10⁻⁶ K⁻¹ |
| Linear expansion, 20 to 200 °C | 17 × 10⁻⁶ K⁻¹ |
| Linear expansion, 20 to 300 °C | 17 × 10⁻⁶ K⁻¹ |
| Linear expansion, 20 to 400 °C | 18 × 10⁻⁶ K⁻¹ |
| Linear expansion, 20 to 500 °C | 18 × 10⁻⁶ K⁻¹ |
| Modulus of elasticity at 200 °C | 186 GPa |
| Modulus of elasticity at 400 °C | 172 GPa |
| Magnetisability | Slight when annealed, magnetic after cold forming |

## 5. Forging, heat treatment and machining

**Forging.** Forgeability is rated good and both open-die forging and drop forging are suitable. Heat slowly to roughly 1150 to 1200 °C and work down to about 900 °C, then cool in air or water. Some mill datasheets set the finishing floor higher, at 930 °C, and on thin sections that is the safer number to work to. Slow heating matters on heavy sections because thermal conductivity is low at 15 W/(m·K), so a fast ramp puts the surface a long way ahead of the core.

**Solution annealing.** Optimum properties follow solution annealing between 1000 and 1100 °C with rapid cooling in air or water. Forgings are solution treated after forging as standard. Keep dwell time short in the 450 to 850 °C range: chromium carbide precipitation is the main metallurgical risk with this grade.

**Machining.** Machinability is moderate, and the grade is rarely chosen where heavy machining is the main operation. The high work-hardening rate combined with low thermal conductivity means the tool must stay below the hardened layer left by the previous pass. Use coated carbide, rigid setups, positive uninterrupted cuts and generous coolant. Dwelling or rubbing will glaze the surface and the next pass will struggle.

Table 7 — Indicative turning parameters, solution annealed, Rm 550 to 650 N/mm².

| Depth of cut | Feed rate | Cutting speed |
|---|---|---|
| 6 mm | 0.5 mm/rev | 130 m/min |
| 3 mm | 0.4 mm/rev | 210 m/min |
| 1 mm | 0.2 mm/rev | 250 m/min |

**Welding.** Weldability is good across TIG, arc and laser beam welding. Preheating is not required and post-weld heat treatment is not mandatory, though a solution treatment after welding is advisable where intergranular attack is a concern. Where filler metal is used, a 308L type consumable is recommended and the interpass temperature should stay below 200 °C. Welding cold-worked material destroys the cold-work strength in and around the weld, which is why welded spring components are uncommon in this grade.

## 6. Corrosion behaviour and its limits

General corrosion resistance is good and polishing improves it noticeably, since surface finish has a strong effect on pitting initiation. Three limits have to be designed around.

1. **Not resistant to intergranular corrosion**, either in the delivery condition or in the sensitized condition. The carbon content allows chromium carbides to form at the grain boundaries, leaving chromium-depleted zones that corrode preferentially.
2. **Not resistant to seawater or sodium chloride.** With a PREN of 16.0 to 23.4, pitting occurs in contact with chlorides. The grade is also susceptible to stress corrosion cracking in chloride and hydroxide environments.
3. **Resistance falls as cold work rises.** The strongest cold-formed conditions are also the least corrosion resistant, so strength and corrosion performance have to be traded against each other.

Against that, the grade performs well in nitric acid, fertiliser compounds, many preservatives and salts, and is resistant to water vapour at room temperature. For sour service, seawater, or any duty requiring certified intergranular corrosion resistance, a stabilised grade such as A182 F321 or A182 F347 is the better starting point.

## 7. Applications

1.4310 suits parts that need high strength after cold work together with reasonable general corrosion resistance. As a spring steel it serves up to 300 °C.

Automotive: corrosion-resisting springs, clips, retainers and formed hardware. Mechanical engineering: compression, tension, return, hook and coil springs, spring washers, flexible connectors. Chemical and nitrogen plant: valve parts, fittings, pump components, acid tanks, absorption towers. Food and beverage: processing equipment, storage vessels, hygienic-service components. Heat transfer: forged flanges, tube sheets, nozzles, exchanger components. Rotating equipment: forged shafts, spindles, gear blanks, rings. Valves and fittings: bodies, seat rings, stems, blocks. Electrical: contact springs and precision formed polished components.

## 8. Forged products in this grade

Every item is forged from a single piece of steel melted on site. No welding, no casting, no purchased billet of unknown origin. Each is produced against your drawing rather than from a fixed catalogue.

Seamless rolled rings, ring-rolled from a punched preform, rectangular or contoured section, OD 50 to 6,000 mm. Forged rings by upset and punch for sections outside the ring-mill envelope. Forged flanges, weld neck, blind, slip-on, socket weld, lap joint and orifice to ASME B16.5, B16.47 or EN 1092-1. Shafts and spindles, stepped, gear, pinion and eccentric, turned up to 14,000 mm between centres. Discs and tube sheets machined to 5,000 mm diameter, proof-machined for volumetric inspection. Sleeves and bushings bored to 1,600 mm diameter by 10,000 mm deep. Forged round, flat and square bars, die blocks and machining blanks. Valve bodies, bonnets, seat rings, stems, nozzles, manifolds and near-net shapes.

## 9. Plant and route for this grade

Stainless grades such as 1.4310 take the electric arc, ladle refining and vacuum oxygen decarburisation route. No remelting step is needed, which puts this grade at the shorter end of the lead-time range.

Table 8 — Relevant works capability.

| Stage | Equipment | Limit |
|---|---|---|
| Melting | Electric arc furnace, ladle furnace, vacuum oxygen decarburisation | 60 t maximum heat |
| Forging | Hydraulic open-die presses, 6,300 t, 4,000 t, 2,000 t | 30 t single piece |
| Ring rolling | Radial-axial mills, 6 m, 3 m, 1 m | OD 50 to 6,000 mm |
| Solution annealing | 14 furnaces, car-bottom and well type | 8,000 x 2,000 x 2,000 mm; 15 m deep wells |
| Machining | Vertical and horizontal lathes, CNC, deep-hole drilling | 5,000 mm swing; 14,000 mm length |
| Minimum order | By weight, no minimum piece count | 10 kg |
| Lead time | No remelting step required for this grade | 20 to 60 days |

**Testing and certification.** Chemistry is verified at the furnace by optical emission spectrometry rather than taken from a supplier certificate, because the steel is melted on site. Tensile testing runs on 600 kN and 300 kN machines, with ultrasonic inspection to ASTM A388 or EN 10228-3, magnetic particle inspection to ASTM E709 where applicable, and metallographic grain size to ASTM E112. Intergranular corrosion testing to ASTM A262 or G28, a common request on this grade given its sensitisation behaviour, is placed with an accredited third-party laboratory and reported alongside the mill certificate.

Table 9 — Documentation.

| Item | Detail |
|---|---|
| Class approvals | CCS, BV, DNV, LR, NK |
| Standard certificate | EN 10204 3.1 mill test certificate |
| Witnessed certificate | EN 10204 3.2, witnessed by BV, DNV, LR, SGS, TUV or your own inspector |
| Traceability | Melt number through forging, heat treatment and machining to shipment |
| Supporting records | Heat-treatment charts, NDT reports, dimensional reports, PMI records |

## 10. Questions we get asked

**What is X10CrNi18-8 steel?**
X10CrNi18-8 is an austenitic chromium-nickel stainless steel with EN material number 1.4310, listed in EN 10088-1, EN 10088-2, EN 10088-3 and EN 10151. It contains 0.05 to 0.15 % C, 16.0 to 19.0 % Cr and 6.0 to 9.5 % Ni. The restricted nickel content leaves the austenite metastable, so the steel work hardens rapidly under cold deformation. That is why the grade is best known as a stainless spring steel.

**What is the American equivalent of X10CrNi18-8?**
AISI 301 (UNS S30100) and AISI 302 (UNS S30200). Other designations are JIS SUS301 and SUS302, BS 301S21 and 302S26, AFNOR Z11CN17-08 and Z12CN18-09, SS 2331, GOST 12Kh18N9, PN 1H18N9, UNE F-3507, AMS 5516, ISO X9CrNi18-8, and the withdrawn DIN designation X12CrNi17-7. The EN composition band is wider than AISI 301 on both chromium and nickel, so the purchase order should state which standard governs.

**Does X10CrNi18-8 contain molybdenum?**
No. EN 10088 permits molybdenum only as a residual at maximum 0.80 %, and it is not added deliberately. Where molybdenum is needed for chloride pitting resistance, specify 904L, a 6Mo austenitic grade or a duplex grade instead.

**What is the forging temperature of X10CrNi18-8 / 1.4310?**
Heat slowly to roughly 1150 to 1200 °C and forge down to about 900 °C, then cool in air or water. Some mill datasheets set the finishing floor higher, at 930 °C. Open-die forging and drop forging are both suitable, and solution annealing at 1000 to 1100 °C follows.

**Is X10CrNi18-8 magnetic?**
Only slightly magnetisable when solution annealed. Cold forming turns part of the metastable austenite into deformation martensite, after which the material responds to a magnet. This is normal for the grade and is not evidence of the wrong material being supplied.

**Is X10CrNi18-8 resistant to intergranular corrosion?**
No, neither in the delivery condition nor in the sensitized condition. Chromium carbides form at the grain boundaries and leave chromium-depleted zones. Limit time in the sensitising range during fabrication, and apply a solution treatment after welding or hot forming.

**Can X10CrNi18-8 be welded?**
Yes. Weldability is good across TIG, arc and laser beam welding. Preheating is not needed and post-weld heat treatment is not mandatory. Where filler is used, a 308L type consumable is recommended with interpass temperature below 200 °C. Welding cold-worked parts removes the cold-work strength locally.

**Is X10CrNi18-8 suitable for seawater?**
No. With a PREN of 16.0 to 23.4 the grade is not resistant to seawater or sodium chloride, and pitting occurs in contact with chlorides. It is also susceptible to stress corrosion cracking in chloride and hydroxide environments.

**Who supplies open-die forgings in X10CrNi18-8?**
Jiangyin Jiangnan Metal Co., Ltd., an integrated melting works and open-die forging factory at No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China. Stainless grades are melted in-house through the electric arc furnace, ladle furnace and vacuum oxygen decarburisation route. Rings roll to 6,000 mm outside diameter and single pieces reach 30 tonnes. Minimum order is 10 kg and lead time runs 20 to 60 days. Telephone +86 189 2135 9659, email sales@steelforgepieces.com.

**What is the minimum order quantity?**
10 kg, with no minimum piece count. A single small part is quotable and so is a one-off large ring. Very small parts are grouped into a batch to share furnace and setup time, so quantity still affects the unit price even though it does not affect whether the job can be taken.

**What do you need in order to quote?**
Six things: the grade or specification, the dimensions or a drawing, the quantity and expected repeat volume, the delivery condition, the heat treatment and testing requirements, and the certification level plus destination port. Sending all six in the first email usually gets a price back within two working days.

## Request a quotation

Jiangyin Jiangnan Metal Co., Ltd.
No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
Telephone, WhatsApp and WeChat: +86 189 2135 9659
Email: sales@steelforgepieces.com
Hours: Monday to Saturday, 08:00 to 17:30 China Standard Time (UTC+8)
Minimum order: 10 kg, no minimum piece count

Customer audits, pre-shipment inspection and third-party witness testing are welcome. Please arrange visits by email in advance so an English-speaking engineer is available.

## Related grades

A182 F321, A182 F347, AISI 321H, AISI 347H, A182 F309, AISI 330, 904L, A182 F44, A182 F51, A182 F53, A182 F55, 17-4 PH, 15-5 PH, 17-7 PH, Nitronic 50, Nitronic 60.

---

Data compiled from EN 10088-1, EN 10088-2:2005 and EN 10088-3:2005 for composition, mechanical properties and delivery conditions; EN 10151:2003 for cold-worked spring conditions; EN ISO 6931-1 for room and elevated temperature proof strength; and published 1.4310 mill datasheets for forging, heat treatment, machining, physical and corrosion data. Plant and equipment figures are our own.

Published by Jiangyin Jiangnan Metal Co., Ltd. Last reviewed 9 October 2026. Figures are given for guidance. Confirm every value against the specification governing your order before design or purchase.