# UNS S35315 Forgings (EN 1.4854 / 353 MA)

**Jiangyin Jiangnan Metal Co., Ltd. forges UNS S35315 seamless rolled rings, flanges, shafts, discs, bars, sleeves and tube sheets to drawing at its melting and open-die forging works in Zhouzhuang Town, Jiangyin City, Jiangsu Province, China.**

UNS S35315 is an austenitic heat-resisting stainless steel with nominally 25 % chromium and 35 % nickel, alloyed with nitrogen and rare earth metals. It carries the European number 1.4854 and is sold commercially as 353 MA, a trademark owned by Outokumpu OY.

The grade exists for high temperature service. High silicon plus a cerium addition give very high oxidation resistance and good scale adhesion under thermal cycling, with a maximum service temperature in air of 1150 °C (2102 °F). The nickel content and a dense chromium oxide also give good resistance to carburisation and nitrogen pick-up.

| Field | Detail |
|---|---|
| UNS | S35315 |
| EN number | 1.4854 |
| Trade name | 353 MA (trademark of Outokumpu OY) |
| Type | Austenitic heat-resisting stainless steel |
| Max service temperature, air | 1150 °C (2102 °F) |
| Tensile strength, minimum | 650 MPa (94 ksi) |
| Proof strength Rp0.2, minimum | 300 MPa (44 ksi) |
| Density | 7.9 g/cm³ (0.28 lb/in³) |
| Supplier | Jiangyin Jiangnan Metal Co., Ltd. |
| Plant | No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China |
| Telephone | +86 189 2135 9659 |
| Email | sales@steelforgepieces.com |
| Page | https://www.steelforgepieces.com/Stainless-Steel/UNS-S35315.html |

## Grade selection warning

UNS S35315 contains no molybdenum, and its maximum temperature for aqueous corrosion service is around 450 °C. It is not a seawater or acid grade. For firewater, subsea pipework or sulphuric acid duty, use a super duplex grade such as ASTM A182 F53 or F55, or a high-alloy austenitic such as 904L.

## Chemical composition

Nominal composition, weight %:

| Element | Nominal |
|---|---|
| Carbon, C | 0.07 |
| Silicon, Si | 1.6 |
| Manganese, Mn | 1.5 |
| Phosphorus, P | ≤ 0.040 |
| Sulphur, S | ≤ 0.015 |
| Chromium, Cr | 25 |
| Nickel, Ni | 35 |
| Nitrogen, N | 0.16 |
| Cerium, Ce | 0.05 |
| Iron, Fe | Balance |

Source: Alleima 353 MA datasheet. The ASTM A240 UNS S35315 data sheet published by Gravity Cast India lists cerium 0.030 to 0.100 %, balance iron.

Cerium enters the melt as misch metal containing roughly 50 % Ce, so the quantity of other rare earth metals is added to the cerium figure.

**Correction to a common error.** A widely copied table lists cerium in this grade as 1.3 %, which duplicates the silicon value in the row above it. The real content is 0.030 to 0.100 %. If a mill certificate shows 1.3 % Ce, query it.

## Mechanical properties

Minimum values, solution annealed, 20 °C:

| Property | Metric | Imperial |
|---|---|---|
| Proof strength Rp0.2 | ≥ 300 MPa | ≥ 44 ksi |
| Proof strength Rp1.0 | ≥ 340 MPa | ≥ 49 ksi |
| Tensile strength Rm | ≥ 650 MPa | ≥ 94 ksi |
| Elongation A (5.65√S₀) | ≥ 40 % | ≥ 40 % |
| Elongation A2" | ≥ 35 % | ≥ 35 % |
| Hardness, Vickers | approx. 160 | approx. 160 |

Typical rather than guaranteed values reported for the annealed grade are 720 to 740 MPa tensile, 300 to 360 MPa yield, 46 to 50 % elongation and Brinell hardness around 190.

Short-term minimum strength at temperature:

| °C | Rp0.2, MPa | Rp1.0, MPa | Rm, MPa |
|---|---|---|---|
| 100 | 228 | 261 | 536 |
| 200 | 195 | 223 | 498 |
| 300 | 166 | 190 | 470 |
| 400 | 152 | 173 | 444 |
| 500 | 143 | 163 | 437 |
| 600 | 138 | 159 | 422 |

Creep strength, average values, MPa:

| °C | 1 %, 10,000 h | 1 %, 100,000 h | Rupture, 10,000 h | Rupture, 100,000 h |
|---|---|---|---|---|
| 550 | 149 | 86 | 206 | 129 |
| 600 | 88 | 52 | 127 | 80 |
| 650 | 54 | 33 | 82 | 52 |
| 700 | 35 | 21 | 56 | 36 |
| 750 | 22 | 14 | 39 | 25 |
| 800 | 15 | 9.7 | 28 | 18 |
| 850 | 10.5 | 6.9 | 20 | 14 |
| 900 | 8 | 5.1 | 15 | 10 |
| 950 | 6 | 3.9 | 11 | 6.7 |
| 1000 | 4.5 | 3.0 | 8 | 4.8 |
| 1050 | 3.5 | 2.3 | 6 | 3.5 |
| 1100 | 2.7 | 1.8 | 4.5 | 2.9 |

Source: Alleima 353 MA datasheet. Average values published for seamless tube.

## Physical properties

| °C | Thermal conductivity, W/m·°C | Specific heat, J/kg·°C | Modulus, GPa | Resistivity, µΩ·m |
|---|---|---|---|---|
| 20 | 11 | 480 | 190 | 1.00 |
| 200 | 15 | 530 | 180 | 1.07 |
| 400 | 18 | 575 | 165 | 1.14 |
| 600 | 22 | 610 | 155 | 1.20 |
| 800 | 25 | 640 | 140 | 1.25 |
| 1000 | 27 | 665 | 130 | 1.30 |
| 1100 | 29 | 680 | 125 | 1.32 |

Mean thermal expansion is 15.5 × 10⁻⁶ /°C over 20 to 100 °C, rising to 18 × 10⁻⁶ /°C over 20 to 1000 °C. Melting range 1330 to 1370 °C.

## Behaviour at high temperature

Oxidation resistance comes from the high silicon content together with the rare earth metal addition, which also improves scale adhesion during temperature cycling and so reduces spalling in furnaces that are repeatedly heated and cooled.

The dense chromium oxide and 35 % nickel give good resistance to carburisation and nitrogen pick-up. In cracked ammonia testing, nitrogen pick-up resistance was similar to Alloy 601. High nickel alloys are generally sensitive to sulphur attack at temperature, but under oxidising conditions a protective oxide forms and sulphur resistance improves.

Maximum service temperature in air is 1150 °C. Service below 950 °C may cause reduced room temperature impact toughness, so the grade suits continuous high temperature duty better than long holds in the intermediate range.

## Heat treatment, welding and forming

Solution annealing: 1100 to 1200 °C (2010 to 2190 °F), 5 to 20 minutes, rapid cooling in air or water.

Stress relieving: 1000 to 1100 °C, 10 to 15 minutes, cooling in air.

Welding: weldability is good, with TIG as first choice. Low thermal conductivity and high thermal expansion mean the welding sequence should be planned to limit distortion. Heat input below 1.0 kJ/mm and interpass temperature below 100 °C (210 °F) are recommended.

| Process | Filler metal |
|---|---|
| TIG / GTAW, MIG / GMAW | ISO 18274 S Ni 6082 / AWS A5.14 ERNiCr-3 |
| MMA / SMAW | ISO 14172 E Ni 6182 / AWS A5.11 ENiCrFe-3 |

Cold bending requires higher deformation forces than conventional stainless steels. Annealing after cold bending is not normally necessary.

## Applications

Documented application areas:

- Ethylene furnace radiant cracking tubes
- EDC furnace tubes
- Waste heat recovery systems in the metallurgical industry, for example recuperators
- Heat treatment furnace internals: muffle tubes, radiant tubes, thermocouple protection tubes, burner components, furnace rollers
- Recuperator tubes in chemical waste and sewage sludge incineration
- Components requiring heat and creep resistance above 550 °C in the iron, steel and non-ferrous industries, the cement industry, engineering and energy conservation plant

Forgings we supply against those duties: seamless rolled rings and retaining rings for furnace rollers and burner assemblies; flanges and tube sheets for recuperators and waste heat exchangers; round bars, shafts and spindles for furnace roller and conveyor drives; discs, blanks and sleeves for burner and muffle components; bushings, nozzles and thermocouple protection hardware.

## Forging, testing and certification

| Item | Detail |
|---|---|
| Melting route | EF, LF and VOD on site, with ESR where the order requires it |
| Product forms | Seamless rolled rings, forged rings, flanges, shafts, discs, tube sheets, bars, blocks, sleeves, bushings, nozzles |
| Condition | Solution annealed, rough machined or proof machined as ordered |
| Minimum order | 10 kg, no minimum piece count |
| Lead time | 20 to 60 days |
| NDT | EN 10228-3, SEP 1921, ASTM A388 |
| Certification | EN 10204 3.1 or 3.2 |

Because the works melts its own steel, the certificate traces a finished part back to its melt number rather than stopping at a purchased billet.

## Questions

**What is UNS S35315?** An austenitic heat-resisting stainless steel with nominally 25 % chromium and 35 % nickel, alloyed with nitrogen and rare earth metals. EN number 1.4854, trade name 353 MA.

**How much cerium does it contain?** 0.030 to 0.100 %, nominal 0.05 %. Published figures of 1.3 % are a copying error.

**What is the maximum service temperature?** 1150 °C (2102 °F) in air. Service below 950 °C may reduce room temperature impact toughness.

**Can it be used in seawater or sulphuric acid?** No. No molybdenum in the composition, and maximum temperature for aqueous corrosion service around 450 °C. Use A182 F53, F55 or 904L for those duties.

**Which filler metal?** ERNiCr-3 for TIG and MIG, ENiCrFe-3 for manual metal arc.

**What is needed to quote?** Drawing or finished dimensions with machining allowance, governing standard, quantity, certification level, NDT standard and acceptance class, and any supplementary testing.

## Data sources

Alleima 353 MA material datasheet; AZoM datasheet for stainless steel grade 353MA; MakeItFrom entry for UNS S35315; ASTM A240 UNS S35315 data sheet published by Gravity Cast India. Where sources disagree, the mill datasheet minima govern and other figures are labelled typical.

353 MA is a trademark owned by Outokumpu OY. Jiangyin Jiangnan Metal Co., Ltd. is an independent forging manufacturer with no affiliation to the trademark holder.

---
