# UNS S31700 (AISI 317) Stainless Steel Forgings

**UNS S31700 is the austenitic stainless steel also designated AISI Type 317, SAE 30317 and Werkstoff 1.4449. It contains 18.0-20.0 % chromium, 11.0-15.0 % nickel and 3.0-4.0 % molybdenum with carbon held to 0.08 % maximum. Forgings in this grade are ordered to ASTM A182 grade F317.**

Type 317 is a modified Type 316 carrying more chromium, nickel and molybdenum. The extra molybdenum raises strength and improves resistance to pitting and crevice corrosion where chlorides are present.

Jiangyin Jiangnan Metal Co., Ltd. melts this grade on site through the electric arc furnace, ladle furnace and vacuum oxygen decarburisation route, then forges, heat treats, machines and tests it in the same works at Jiangyin, Jiangsu, China. Rings roll to 6,000 mm outside diameter and single pieces reach 30,000 kg.

Source page: https://www.steelforgepieces.com/Stainless-Steel/UNS-S31700.html
Last reviewed: 2026-10-05

## Grade identification

| Field | Value |
|---|---|
| UNS | S31700 |
| AISI | Type 317 |
| Forging specification | ASTM A182 / ASME SA-182 grade F317 |
| Werkstoff | 1.4449 |
| SAE | 30317, J405 (30317) |
| Microstructure | Austenitic, not hardenable by heat treatment |
| Annealing | 1010-1121 C (1850-2050 F) followed by cooling |
| Melting route | EF, LF, VOD. ESR available |
| Certification | EN 10204 type 3.1 or type 3.2 |

## Chemical composition, weight %

| Element | ASTM A182 F317 limit | Typical |
|---|---|---|
| Carbon, C | 0.08 max | 0.08 |
| Chromium, Cr | 18.0-20.0 | 19 |
| Nickel, Ni | 11.0-15.0 | 13 |
| Molybdenum, Mo | 3.0-4.0 | 3.50 |
| Manganese, Mn | 2.00 max | 2 |
| Silicon, Si | 1.00 max | 1 |
| Phosphorus, P | 0.045 max | 0.045 |
| Sulfur, S | 0.030 max | 0.030 |
| Iron, Fe | Balance | 61 |

Limits per ASTM A182 grade symbol F317. Typical values per the AZoM Grade 317 data sheet. The mill certificate states the actual heat analysis.

### S31700 against S31703 (317L)

Chromium, nickel and molybdenum ranges are identical. Carbon is the difference: 0.08 % maximum for 317, 0.03 % maximum for 317L. Lower carbon in 317L holds back carbide precipitation in the weld heat-affected zone, so welded vessels are usually specified in 317L while 317 keeps a small strength advantage. The choice has to be made before the heat is booked.

## Mechanical properties

Specified minimums and typical values are not interchangeable. Buy to the minimums, expect the typicals.

| Property | ASTM A182 F317 minimum | Typical, annealed |
|---|---|---|
| Tensile strength | 515 MPa (75 ksi) | 620 MPa (89,900 psi) |
| Yield strength, 0.2 % offset | 205 MPa (30 ksi) | 275 MPa (39,900 psi) |
| Elongation in 50 mm or 4D | 30 % | 45 % |
| Reduction of area | 50 % | not stated |
| Hardness, Rockwell B | to order | 85 HRB |
| Modulus of elasticity | not specified | 193 GPa (27,993 ksi) |
| Poisson's ratio | not specified | 0.27-0.30 |

Heavy sections test lower than thin ones at the same chemistry. Agree test location and acceptance values at enquiry stage.

## Physical and thermal properties

| Property | Metric | Imperial |
|---|---|---|
| Density | 8.0 g/cm3 | 0.289 lb/in3 |
| Melting point | 1370 C | 2550 F |
| Thermal conductivity at 100 C | 16.3 W/m.K | 113 BTU.in/hr.ft2.F |
| Thermal expansion, 0-100 C | 16 um/m.C | 8.89 uin/in.F |

## Designations and product specifications

| Category | Designation |
|---|---|
| UNS | S31700 |
| AISI / SAE | Type 317, SAE 30317, SAE J405 (30317) |
| German | DIN / Werkstoff 1.4449 |
| Forgings and forged fittings | ASTM A182 grade F317, ASTM A403, ASME SA403, ASTM A473 |
| Bar, billet, wire | ASTM A276, A314, A479, A478, A580 |
| Plate, sheet, strip | ASTM A240, ASME SA240, ASTM A167 |
| Pipe and tube | ASTM A213, A249, A269, A312, A409, A511, A554, A632, A813, A814; ASME SA249, SA312, SA409 |
| Military and federal | QQ S763, MIL-S-862 |

## Forging, heat treatment and machining

**Melting.** Electric arc furnace, ladle furnace refining and vacuum oxygen decarburisation, maximum heat 60 t. Protective-atmosphere electroslag remelting on the 3 t or 6 t furnace where a cleaner ingot or better transverse properties are required.

**Hot working.** 1149-1260 C (2100-2300 F). Do not work below 927 C (1700 F). Anneal after hot work to restore corrosion resistance.

**Heat treatment.** Anneal at 1010-1121 C (1850-2050 F) and cool. The grade does not respond to hardening heat treatment; strength above the annealed level comes only from cold work. Fourteen furnaces on site, including car-bottom chambers to 8,000 mm long and two pit furnaces 15,000 mm deep for vertical treatment of long shafts.

**Cold working.** Stamping, shearing, drawing and heading all apply. Anneal afterwards to reduce internal stress.

**Machining.** Tougher than Type 304, so use chip breakers and avoid constant feeds at low speed. On site: vertical turning to 5,000 mm swing, horizontal turning to 14,000 mm, CNC turning and milling, deep-hole drilling to 1,600 mm diameter by 10,000 mm.

**Welding.** Fusion and resistance methods with AWS E317, ER317 or 317L filler. Oxyacetylene welding is not recommended.

## Corrosion behaviour

S31700 resists atmospheric corrosion and performs in moderately oxidising and reducing conditions. Its 3-4 % molybdenum, higher than Type 316 carries, is the main contributor to pitting and crevice resistance in chloride-bearing service.

In acid duty, austenitic stainless steels of the 317 family are considerably more resistant than conventional chromium-nickel types to sulfuric acid, and resistance rises with molybdenum content. ATI reports 317L, 317LM and 317LMN as resistant to sulfuric acid up to 5 % concentration at temperatures as high as 49 C, with better behaviour below 38 C.

Every austenitic grade loses ground as chloride level and temperature rise together. Where the duty exceeds what 317 will carry, a duplex or super-austenitic grade is the right answer rather than a thicker 317 section. The same works forges A182 F51, F53, F55, F44, 904L and Sanicro 28.

## Forged product forms

- Seamless rolled rings, rolled on 1 m, 3 m and 6 m radial-axial mills to 6,000 mm outside diameter.
- Forged rings from 50 mm outside diameter, including retaining rings, gear ring blanks and valve seat rings.
- Flanges: weld neck, blind, slip-on, socket weld, lap joint, orifice, anchor, girth, swivel, long weld neck, to ASME B16.5 and B16.47.
- Round, flat and square bar, die blocks and mould blocks.
- Discs, tube sheets and covers to 5,000 mm machined diameter, proof-machined for volumetric inspection.
- Shafts, spindles, crankshafts and rolls turned to 14,000 mm.
- Sleeves, bushings, couplings and bored cylinders to 1,600 mm diameter by 10,000 mm.
- Valve and wellhead parts: bodies, bonnets, blocks, stems, seat rings, spools, nozzles, manifolds.

**Typical service.** Published application areas for Grade 317 are pulp and paper plant, textile processing and chemical equipment. In forged form: digesters, liquor tanks and paper machine parts, absorber towers, scrubbers, stack liners, recuperators, heat exchangers, boilers, pressure vessels, slurry tanks, pumps, valves, refinery and catalytic recovery systems, waste treatment and thermal oxidisers, pharmaceutical and biochemical process equipment.

## Size envelope

| Product | Limit | Set by |
|---|---|---|
| Seamless rolled rings | to OD 6,000 mm | 6 m radial-axial ring mill |
| Rings, small | from OD 50 mm | Upset-and-punch route |
| Shafts | to 14,000 mm turned length | C61160 lathe; 15 m pit furnace |
| Discs, tube sheets, blocks | to 5,000 mm diameter | 5,000 mm vertical turning lathe |
| Bored cylinders, hollow shafts | to 1,600 mm dia x 10,000 mm | CNC deep-hole drilling machine |
| Single piece weight | to 30,000 kg | 60 t heat, 6,300 t press |
| Minimum order | 10 kg | No minimum piece count |
| Lead time | 20 to 60 days | Grade, section, heat treatment cycle |

## Testing and certification

Ultrasonic examination to the standard named on the order. EN 10228-4 is the European standard covering austenitic and austenitic-ferritic stainless steel forgings; EN 10228-3 covers ferritic and martensitic forgings and does not apply here. ASTM A388 covers contact pulse-echo examination of steel forgings by straight and angle beam techniques including the distance-gain-size method.

Documents are issued as EN 10204 type 3.1, signed by the works inspection department, or type 3.2 where an independent surveyor witnesses testing and counter-signs. Positive material identification, dye penetrant examination, impact testing, intergranular corrosion testing to ASTM A262, hardness survey and dimensional reports can be added. The works holds CCS, BV, DNV, LR and NK approvals. Because the steel is melted here, the certificate traces a part back to its melt number rather than to a purchased billet.

## Frequently asked questions

**What is UNS S31700 stainless steel?**
UNS S31700 is the austenitic stainless steel also designated AISI Type 317, SAE 30317 and Werkstoff 1.4449, containing 18.0-20.0 % chromium, 11.0-15.0 % nickel and 3.0-4.0 % molybdenum with carbon at 0.08 % maximum. It is a modified Type 316 with more chromium, nickel and molybdenum, which raises strength and resistance to pitting and crevice corrosion. Forgings are ordered to ASTM A182 grade F317.

**What are the ASTM A182 F317 minimum mechanical properties?**
515 MPa (75 ksi) minimum tensile, 205 MPa (30 ksi) minimum yield, 30 % minimum elongation in 50 mm or 4D, 50 % minimum reduction of area. Annealed material normally tests around 620 MPa, 275 MPa, 45 % and 85 HRB.

**What is the difference between 317 and 317L?**
Carbon. 317 permits 0.08 % maximum, 317L permits 0.03 % maximum. Chromium, nickel and molybdenum are the same. 317L is preferred for welded fabrication, 317 keeps a small strength advantage.

**How is UNS S31700 heat treated?**
Annealed at 1010-1121 C (1850-2050 F) then cooled. Not hardenable by heat treatment, only by cold work. Hot worked at 1149-1260 C, not below 927 C.

**Can UNS S31700 be welded?**
Yes, by fusion and resistance methods with AWS E317, ER317 or 317L filler. Oxyacetylene welding is not recommended.

**What size forgings can you produce?**
Rings to 6,000 mm outside diameter, presses to 6,300 t, single pieces to 30,000 kg from 60 t heats. Shafts to 14,000 mm, discs to 5,000 mm diameter, bored hollows to 1,600 mm by 10,000 mm. Minimum order 10 kg, lead time 20 to 60 days.

**What certification is supplied?**
EN 10204 type 3.1 or type 3.2, with ultrasonic examination to ASTM A388 or EN 10228-4.

**How do I get a price?**
Price depends on the drawing, the finished weight and the quantity, so there is no list price. Send a drawing or finished dimensions, the specification, the quantity and any testing requirements to sales@steelforgepieces.com or call +86 189 2135 9659.

## Contact

Jiangyin Jiangnan Metal Co., Ltd., open-die forging works, established 1997.
No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China.
Telephone +86 189 2135 9659. Email sales@steelforgepieces.com.

Grade data is published for guidance. The purchase order specification and the mill certificate for the supplied heat govern.