# UNS S31651 (AISI 316N) Open-Die Forgings: Composition, Properties and Product Range

**Source:** https://www.steelforgepieces.com/Stainless-Steel/UNS-S31651.html
**Supplier:** Jiangyin Jiangnan Metal Co., Ltd., open-die forging factory, Jiangyin, Jiangsu, China
**Address:** No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
**Telephone / WhatsApp / WeChat:** 0086-189-2135-9659
**Email:** sales@steelforgepieces.com
**Published:** 2019-03-12 | **Last reviewed:** 2026-09-21

---

## Summary

UNS S31651 is the Unified Numbering System number for AISI Type 316N, a nitrogen-strengthened, molybdenum-bearing austenitic stainless steel. The composition limits are 16.0 to 18.0 % chromium, 10.0 to 14.0 % nickel, 2.00 to 3.00 % molybdenum and 0.10 to 0.16 % nitrogen, with carbon held to 0.08 % maximum and iron as the balance.

Nitrogen strengthens the alloy by interstitial solid solution. It lifts the specified minimum yield strength from 205 MPa (30 ksi) for Type 316 to 240 MPa (35 ksi), and the minimum tensile strength from 515 MPa to 550 MPa (80 ksi). Carbon is not raised to achieve this, so weldability and chloride behaviour stay close to standard 316. The higher minimums give a higher ASME allowable stress, which lets a designer use a thinner wall on a flange hub, valve body or vessel nozzle.

Jiangyin Jiangnan Metal Co., Ltd. forges UNS S31651 into round, square and flat bars, hollow bars and sleeves, seamless rolled rings, discs, blocks, shafts, spindles and flanges. Material is supplied solution annealed with EN 10204 3.1 or 3.2 certification.

## Key facts

| Item | Value |
|---|---|
| UNS number | S31651 |
| Common name | AISI 316N |
| Forging specification | ASTM A182 / ASME SA-182 Grade F316N |
| Tensile strength, minimum | 550 MPa (80 ksi) |
| Yield strength 0.2 %, minimum | 240 MPa (35 ksi) |
| Elongation in 50 mm, minimum | 30 % |
| Reduction of area, minimum | 50 % |
| Density | 7.98 g/cm3 |
| PREN | 24 to 31, typically 27 |
| Solution annealing | 1040 to 1100 degrees C, rapid quench |
| Delivery condition | Solution annealed |

---

## 1. What UNS S31651 is and why nitrogen is added

UNS S31651 sits in the 18-8 austenitic family, on the molybdenum-bearing 316 branch. Molybdenum at 2 to 3 % holds the passive film against chloride attack. Chromium at 16 to 18 % forms that film. Nickel at 10 to 14 % keeps the structure fully austenitic and tough down to cryogenic temperature. What separates S31651 from plain 316 is a controlled nitrogen range of 0.10 to 0.16 %.

Nitrogen dissolves in the austenite lattice as an interstitial. Per weight percent it is one of the strongest solid solution strengtheners available in stainless steel, roughly ten times more effective than nickel or molybdenum. It does not form chromium carbides at grain boundaries the way carbon does, so the added strength costs nothing in intergranular corrosion resistance. Nitrogen also adds to the pitting resistance equivalent, and it makes the austenite more stable against strain-induced martensite during cold work.

Design codes are where this shows up in practice. ASME allowable stresses come from the specified minimum yield and tensile values, so moving from 205 MPa to 240 MPa minimum yield lets a designer take wall thickness out of a flange hub, valve body or nozzle. On a large forging, removing 10 % of the wall can take several hundred kilograms out of the part, which shows up in material cost, machining hours and freight.

**Naming.** UNS S31651, AISI Type 316N, ASTM A182 Grade F316N, ASME SA-182 F316N, JIS SUS316N and GB/T 06Cr17Ni12Mo2N all designate the same alloy. Which specification you order to depends on the product form and the code the component is built to.

## 2. Chemical composition limits of UNS S31651

Specification window per ASTM A182/A182M Grade F316N and ASTM A240 Type 316N. Weight percent, heat analysis. Product analysis tolerances apply per the governing standard.

| Element | Symbol | Minimum | Maximum | Role in the alloy |
|---|---|---|---|---|
| Carbon | C | – | 0.080 | Strength. Held low to limit carbide sensitisation |
| Manganese | Mn | – | 2.00 | Deoxidiser. Raises nitrogen solubility |
| Phosphorus | P | – | 0.045 | Residual. Restricted for hot ductility |
| Sulfur | S | – | 0.030 | Residual. Restricted for forgeability |
| Silicon | Si | – | 0.75 | Deoxidiser. Aids oxidation resistance |
| Chromium | Cr | 16.00 | 18.00 | Forms the passive chromium oxide film |
| Nickel | Ni | 10.00 | 14.00 | Stabilises austenite. Low-temperature toughness |
| Molybdenum | Mo | 2.00 | 3.00 | Pitting and crevice corrosion resistance |
| Nitrogen | N | 0.10 | 0.16 | Solid solution strengthening. Raises PREN |
| Iron | Fe | Balance, approx. 61.9 to 71.9 | | Matrix |

**Melt practice.** Billet for UNS S31651 forgings is procured to AOD, or AOD plus ESR where the specification calls for it. Nitrogen recovery is verified by product analysis on the finished forging rather than by the ladle certificate alone, because nitrogen can be lost during long soaking at forging temperature. A narrower nitrogen band, for example 0.12 to 0.16 % for allowable stress reasons, is agreed at order entry and stated on the mill test certificate.

## 3. Mechanical properties of UNS S31651 forgings

Specified minimum room-temperature requirements for forged UNS S31651 in the solution-annealed condition, per ASTM A182/A182M Grade F316N. The typical column reflects values reached on forged sections up to about 200 mm ruling section.

| Property | ASTM A182 F316N minimum | Typical as produced |
|---|---|---|
| Tensile strength, Rm | 550 MPa (80 ksi) | 590 to 680 MPa |
| Yield strength, Rp0.2 | 240 MPa (35 ksi) | 270 to 340 MPa |
| Elongation in 50 mm, A | 30 % | 40 to 55 % |
| Reduction of area, Z | 50 % | 60 to 75 % |
| Hardness | 217 HBW max (96 HRB max) | 150 to 190 HBW |
| Charpy V impact at -196 C | Not required by A182 | 80 J and above, on request |
| Modulus of elasticity, E | – | 193 to 200 GPa |
| Poisson's ratio | – | 0.27 to 0.30 |

### Strength at temperature

Like all austenitic stainless steels, UNS S31651 gives up a large part of its room-temperature yield strength as temperature rises, then holds a broad plateau. The nitrogen contribution carries across that plateau, which is why 316N carries higher ASME Section II Part D allowable stresses than 316 over most of the useful range.

| Temperature | 100 C | 200 C | 300 C | 400 C | 500 C |
|---|---|---|---|---|---|
| Rp0.2, MPa, approx. | 205 | 175 | 160 | 150 | 145 |

These figures are for preliminary screening only. Allowable stress values for pressure-retaining components must be taken from ASME BPVC Section II Part D, EN 13445-2 or the governing design code for the actual product form and thickness.

## 4. Physical and thermal properties

| Property | Metric | Imperial |
|---|---|---|
| Density | 7.98 g/cm3 | 0.288 lb/in3 (498 lb/ft3) |
| Melting range | 1370 to 1400 C | 2500 to 2550 F |
| Modulus of elasticity at 20 C | 193 to 200 GPa | 28 to 29 x 10^6 psi |
| Thermal conductivity at 100 C | 15 W/m·K | 104 BTU·in/h·ft2·F |
| Specific heat capacity at 20 C | 500 J/kg·K | 0.12 BTU/lb·F |
| Thermal expansion, 0 to 100 C | 16.0 µm/m·K | 8.9 µin/in·F |
| Thermal expansion, 0 to 500 C | 17.5 µm/m·K | 9.7 µin/in·F |
| Electrical resistivity at 20 C | 0.74 µΩ·m | approx. 2.4 % IACS |
| Relative magnetic permeability | below 1.02, annealed | Non-magnetic |

Two of these numbers cause most fabrication trouble. Thermal conductivity of 15 W/m·K is about a third that of carbon steel, so heat does not leave the cut zone during machining. Thermal expansion of 16.0 µm/m·K is roughly 40 % higher than carbon steel, so weld shrinkage and distortion on large assemblies are greater, and machining allowances on long shafts have to account for it.

## 5. Corrosion resistance and PREN of UNS S31651

    PREN = %Cr + 3.3 x %Mo + 16 x %N

- Minimum composition, 16.0 Cr / 2.00 Mo / 0.10 N: PREN about 24.2
- Mid-range heat, 17.0 Cr / 2.50 Mo / 0.13 N: PREN about 27.3
- Maximum composition, 18.0 Cr / 3.00 Mo / 0.16 N: PREN about 30.5

For comparison, standard Type 316 with no nitrogen addition falls around 24 to 25, Type 304 around 18 to 20, and super-austenitic A182 F44 (UNS S31254, 6Mo) around 43. UNS S31651 therefore sits between plain 316 and the high-alloy grades.

### Where UNS S31651 works well

- Sulfuric, phosphoric and organic acids at moderate concentration and temperature, where molybdenum is the deciding element.
- Neutral and mildly acidic chloride waters, including seawater at ambient temperature for intermittent service.
- Mildly sour hydrocarbon streams, subject to NACE MR0175 and ISO 15156 qualification of the specific component.
- Cryogenic duty to -196 C, where austenite stability keeps impact toughness high and the nitrogen strengthening is retained.

### Where it should not be used

- **Hot chloride stress corrosion cracking.** Above roughly 60 C in chloride service under tensile stress, all 300-series austenitics including 316N are at risk. Duplex grades such as A182 F51 (UNS S31803) or A182 F53 (UNS S32750) are the correct choice there.
- **Warm seawater or concentrated brine.** Specify 904L or a 6Mo grade instead.
- **Heavy welded sections that will sit between 425 and 815 C and cannot be re-solution annealed.** Specify 316L or 316LN (UNS S31653), which cap carbon at 0.030 %.

## 6. International equivalent grades for UNS S31651

| Standard or region | Designation | Match | Note |
|---|---|---|---|
| UNS, USA | S31651 | Exact | Reference designation |
| AISI / ASTM, USA | Type 316N | Exact | Grade name |
| ASTM A182 / ASME SA-182 | F316N | Exact | Forged flanges, fittings, valves |
| ASTM A240 | 316N | Exact | Plate, sheet, strip |
| ASTM A276 / A479 | 316N | Exact | Bars and shapes |
| JIS, Japan | SUS 316N | Exact | JIS G 4303, G 4304 |
| GB/T, China | 06Cr17Ni12Mo2N (formerly 0Cr17Ni12Mo2N) | Exact | GB/T 1220, GB/T 20878 |
| EN, Europe | 1.4406 / X2CrNiMoN17-11-2; 1.4429 / X2CrNiMoN17-13-3 | **Nearest only** | Both are 316LN: nitrogen alloyed, carbon 0.030 % max. No exact EN counterpart to 316N exists |
| AFNOR, France | Z3 CND 17-12 Az | Nearest | Low-carbon nitrogen grade |
| BS, UK, withdrawn | 316 S 62 | Nearest | Superseded by EN designations |
| ISO | X2CrNiMoN17-12-2 | Nearest | ISO 15510 |

**Substitution warning.** There is no exact European equivalent to UNS S31651. Both 1.4406 and 1.4429 restrict carbon to 0.030 % maximum, which makes them 316LN rather than 316N. Substituting them is usually conservative, since lower carbon improves sensitisation resistance while nitrogen keeps the strength, but it remains a deviation that the design authority has to approve in writing before material is released.

## 7. UNS S31651 against 316, 316L and 316LN

| Grade | UNS | C max, % | N, % | Yield min, MPa | Tensile min, MPa | Best suited to |
|---|---|---|---|---|---|---|
| 316 | S31600 | 0.08 | – | 205 | 515 | General corrosion service, machined parts |
| 316L | S31603 | 0.030 | – | 170 to 205 | 485 to 515 | Heavily welded assemblies, no post-weld anneal |
| **316N** | **S31651** | **0.08** | **0.10 to 0.16** | **240** | **550** | **Pressure parts needing higher allowable stress** |
| 316LN | S31653 | 0.030 | 0.10 to 0.16 | 240 | 550 | Welded pressure parts, nuclear service |

Selection follows from the fabrication route. A component machined from a forging and welded lightly or not at all gets the strength most cheaply from 316N. A component welded in heavy section that cannot be re-solution annealed afterwards should move to 316LN and accept the premium for lower carbon. Where neither strength nor heavy welding is the driver, plain 316 or 316L is enough.

## 8. UNS S31651 forged product forms and size range

Jiangyin Jiangnan Metal produces UNS S31651 by open-die forging and seamless ring rolling. Open-die forging is used instead of casting or plate fabrication because the reduction ratio breaks down the as-cast dendritic structure, closes porosity and aligns grain flow with the loaded direction.

| Product form | Size range |
|---|---|
| Round, square, flat and hex bars | Round 80 to 1,200 mm diameter; lengths to 8,000 mm; black forged, rough turned, or peeled and polished |
| Hollow bars, sleeves, bushings, cylinders, casings, shells | OD 150 to 2,500 mm, ID from 100 mm |
| Seamless rolled rings | OD 200 to 4,000 mm, wall from 40 mm, height to 1,500 mm; rectangular and contour-rolled |
| Discs, blocks and plates | Discs to 3,000 mm diameter; blocks and slabs to 800 mm thickness |
| Shafts and spindles | Straight and stepped, to 8,000 mm length, integral collars and flanged ends |
| Flanges and near-net shapes | Forged flange blanks to ASME B16.5 and B16.47; custom preforms to drawing |

Minimum order quantity is one piece, including a single prototype forging. Material can be supplied black forged, rough machined to your allowance, or finish machined to drawing.

## 9. Forging and heat-treatment practice for UNS S31651

| Operation | Parameter | Reason |
|---|---|---|
| Pre-heat and soak | Slow to 850 C, then to forging heat | Low thermal conductivity. Avoids thermal cracking in heavy sections |
| Forging start temperature | 1150 to 1230 C | Upper limit avoids incipient melting and delta ferrite |
| Finish forging temperature | Not below 925 C | Prevents carbide precipitation and hot tearing on the last blows |
| Minimum reduction ratio | 3:1 typical, 4:1 for critical parts | Breaks down as-cast structure and closes centreline porosity |
| Cooling after forging | Air cool | No transformation hardening in austenitic steel |
| Solution annealing | 1040 to 1100 C, soak, rapid water quench | Dissolves carbides and restores full corrosion resistance |
| Quench delay | As short as practicable through 815 to 425 C | The sensitisation band. Slow cooling here precipitates Cr23C6 |
| Stress relief | Not normally applied | Any treatment in the sensitisation band would undo the anneal |
| Descaling | Pickle and passivate | Removes forge scale and free iron from the surface |

### Machining guidance

UNS S31651 work-hardens faster than 316 because nitrogen raises the work-hardening rate. Use rigid setups, positive rake carbide tooling, moderate surface speed and a heavy uninterrupted feed. Feeding too lightly lets the tool ride on and burnish the work-hardened layer, which destroys tool life. Use flood coolant and do not allow the tool to dwell in the cut.

## 10. Applications of UNS S31651 forgings by industry

- **Oil, gas and petrochemical.** Weld neck and blind flanges, valve bodies and bonnets, wellhead components, separator nozzles and pipeline fittings to ASTM A182 F316N.
- **Chemical process plant.** Reactor nozzles, agitator shafts, pump casings and impellers, heat exchanger tubesheets and channel covers in sulfuric, phosphoric and organic acid duty.
- **Marine and desalination.** Pump shafts and sleeves, propeller shaft components, seawater valve internals and high-pressure pump parts for reverse osmosis trains.
- **Power generation.** Pressure boundary fittings, pump and valve internals, and support hardware where a nitrogen-strengthened 316 variant is the code-specified choice.
- **Pulp, paper and food processing.** Digester and bleach plant hardware, roll journals, and hygienic pressure vessel components needing a smooth passivated surface.
- **Cryogenic and LNG.** Valve bodies, flanges and pump parts for service to -196 C.

## 11. Testing, NDT and certification

| Test | Method or standard | Scope |
|---|---|---|
| Chemical analysis | Optical emission spectrometry, nitrogen by inert gas fusion | Heat and product analysis |
| Tensile test | ASTM A370, ISO 6892-1 | Per heat and heat-treatment lot |
| Hardness | ASTM E10 Brinell | Each piece |
| Impact test | ASTM A370 Charpy V, ambient or cryogenic | On request |
| Intergranular corrosion | ASTM A262 Practice E (Strauss) | On request. Practice A, B and C available |
| Ultrasonic examination | ASTM A388, EN 10228-3 | Standard on rings, discs and shafts |
| Liquid penetrant examination | ASTM E165, EN 10228-2 | Machined surfaces, on request |
| Positive material identification | Portable XRF | On request, marked per piece |
| Grain size and microstructure | ASTM E112 | On request |
| Ferrite content | Feritscope or metallographic | On request |
| Dimensional report | Per customer drawing | Each piece |
| Certification | EN 10204 3.1 standard; 3.2 with TUV, SGS, BV, Lloyd's Register or customer inspector | Every order |

Heat traceability runs from the billet certificate through forging travellers, heat-treatment charts and final release, so any piece can be traced back to its heat number and anneal cycle.

## 12. How to specify a UNS S31651 enquiry

1. **Grade and specification.** UNS S31651, and the governing standard: ASTM A182 F316N, ASTM A479 316N, or your own material specification number.
2. **Product form and dimensions.** Bar, ring, disc, shaft, sleeve or flange, with finished dimensions and the machining allowance to be left on.
3. **Quantity and delivery date.** Piece count and required arrival date, not ex-works date.
4. **Delivery condition.** Black forged, rough turned, or finish machined to drawing.
5. **Testing requirements.** Tensile, impact temperature, ASTM A262 practice, UT acceptance class, PMI, witnessed or not.
6. **Certification.** EN 10204 3.1 or 3.2, and which third party if 3.2.
7. **Marking, packing and destination port.** Heat number marking method, and whether seaworthy wooden cases are required.

## 13. Frequently asked questions about UNS S31651

**What is UNS S31651?**
UNS S31651 is the Unified Numbering System number for AISI Type 316N, a nitrogen-strengthened molybdenum-bearing austenitic stainless steel. The composition limits are 16.0 to 18.0 % chromium, 10.0 to 14.0 % nickel, 2.00 to 3.00 % molybdenum, 0.10 to 0.16 % nitrogen and 0.08 % carbon maximum, with iron as the balance. In forged form it is ordered as ASTM A182 or ASME SA-182 Grade F316N.

**Is UNS S31651 the same as 316N?**
Yes. UNS S31651, AISI 316N, Type 316N and ASTM A182 F316N all name the same alloy. UNS S31651 is the numeric designation, 316N is the AISI and ASTM grade name, and F316N is the forging grade symbol used in ASTM A182.

**What is the difference between 316N and 316L?**
316N (UNS S31651) contains 0.10 to 0.16 % nitrogen and allows carbon up to 0.08 %, giving a specified minimum yield strength of 240 MPa. 316L (UNS S31603) has no deliberate nitrogen addition and holds carbon to 0.030 %, giving a minimum yield of 205 MPa. Use 316N when higher code allowable stress is the driver. Use 316L when resistance to weld sensitisation is the driver. 316LN (UNS S31653) gives both.

**What ASTM standard covers UNS S31651 forgings?**
Forged UNS S31651 is supplied to ASTM A182/A182M Grade F316N, or the ASME Boiler and Pressure Vessel Code equivalent SA-182 F316N, covering forged flanges, fittings, valves and parts for high-temperature service. Plate and sheet fall under ASTM A240 Type 316N. Bars and shapes fall under ASTM A276 and A479.

**What is the PREN of UNS S31651?**
Using PREN = %Cr + 3.3 x %Mo + 16 x %N, UNS S31651 gives about 24 at minimum composition and about 31 at maximum, with a typical heat around 27. That is several points above plain Type 316, entirely because of the nitrogen term.

**Is UNS S31651 magnetic?**
No. In the solution-annealed condition it is fully austenitic and non-magnetic, with relative permeability normally below 1.02. Nitrogen and nickel stabilise the austenite, so it resists strain-induced martensite better than Type 304. Heavy cold work can produce a slight local magnetic response.

**Can UNS S31651 be welded?**
Yes. It welds by GTAW, SMAW, GMAW and SAW without preheat. ER316L and E316L-16 consumables are common. Where the weld metal has to match the nitrogen-enhanced strength of the base material, a nitrogen-alloyed filler such as ER316LMn is specified. Because carbon can reach 0.08 %, long exposure between 425 and 815 C can sensitise heavy sections, so 316LN is preferred for thick welded assemblies that cannot be re-solution annealed.

**What is the EN or DIN equivalent of UNS S31651?**
There is no exact EN equivalent. The closest grades are 1.4406 (X2CrNiMoN17-11-2) and 1.4429 (X2CrNiMoN17-13-3), both nitrogen alloyed but with carbon restricted to 0.030 % maximum, which makes them 316LN rather than 316N. Confirm with your design authority before substituting.

**What is the maximum service temperature of UNS S31651?**
Oxidation resistance in air is adequate to roughly 870 C in continuous service and about 925 C intermittently. For pressure-retaining components, ASME Section II Part D lists allowable stresses well into the 800 C range, but with carbon permitted to 0.08 % long exposure between 425 and 815 C risks carbide sensitisation. Where long-term service falls in that band, specify 316LN.

**What forged shapes are available in UNS S31651?**
Jiangyin Jiangnan Metal supplies UNS S31651 as forged round, square, rectangular, flat and hexagonal bars, hollow bars, sleeves, bushings, cylinders, casings and shells, seamless rolled rings, forged rings, discs, blocks and plates, and shafts, spindles and flanges. Minimum order quantity is one piece.

**What certification is supplied?**
Every order ships with an EN 10204 3.1 mill test certificate as standard, covering heat chemistry, mechanical results, the solution-annealing record, the dimensional report and NDT results. EN 10204 3.2 with third-party inspection by TUV, SGS, BV, Lloyd's Register or your own inspector is available on request.

**What is the lead time for UNS S31651 forgings?**
Lead time depends on size, whether billet is in stock, heat-treatment lot scheduling and the testing scope. Send dimensions, quantity and test requirements to sales@steelforgepieces.com and a date will be confirmed with the quotation.

---

## Contact

**Jiangyin Jiangnan Metal Co., Ltd.**, Open-Die Forging Factory
No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
Telephone / WhatsApp / WeChat: 0086-189-2135-9659
Email: sales@steelforgepieces.com
Web: https://www.steelforgepieces.com/

## Related grades

- A182 F316L, low-carbon 316: https://www.steelforgepieces.com/Stainless-Steel/A182-F316L.html
- A182 F347, stabilised grade: https://www.steelforgepieces.com/Stainless-Steel/A182-F347.html
- A182 F44 (S31254), 6Mo austenitic: https://www.steelforgepieces.com/Stainless-Steel/A182-F44.html
- A182 F51 (S31803), duplex: https://www.steelforgepieces.com/Stainless-Steel/A182-F51.html
- A182 F53 (S32750), super duplex: https://www.steelforgepieces.com/Stainless-Steel/A182-F53.html
- 904L, high-alloy austenitic: https://www.steelforgepieces.com/Stainless-Steel/904L.html
- Nitronic 50, high strength austenitic: https://www.steelforgepieces.com/Stainless-Steel/Nitronic-50.html
- Incoloy 825: https://www.steelforgepieces.com/Nickel-Alloy/Incoloy-825.html

## References

- ASTM A182/A182M, Standard Specification for Forged or Rolled Alloy and Stainless Steel Pipe Flanges, Forged Fittings, and Valves and Parts for High-Temperature Service
- ASTM A240/A240M, Standard Specification for Chromium and Chromium-Nickel Stainless Steel Plate, Sheet, and Strip for Pressure Vessels
- ASTM A276, A479, Stainless steel bars and shapes
- ASME Boiler and Pressure Vessel Code, Section II, Part D, Properties
- EN 10204, Metallic products: Types of inspection documents

*Technical data on this page is for guidance. Verify against the governing standard before design use.*