# UNS S31635 Forgings (316Ti / EN 1.4571)

**UNS S31635 is a titanium-stabilised, molybdenum-bearing austenitic stainless steel of nominal 16Cr-12Ni-2Mo-Ti composition. It is designated 316Ti in the AISI system and 1.4571 or X6CrNiMoTi17-12-2 in EN.**

Titanium of at least five times the combined carbon and nitrogen content binds both elements as Ti(C,N), keeping chromium in solution at the grain boundaries instead of letting it form chromium carbides. Welds and parts held in the 450 to 850 C sensitisation range therefore keep their intergranular corrosion resistance without a post-weld anneal.

Supplied by Jiangyin Jiangnan Metal Co., Ltd., an integrated melting works and open-die forge in Jiangyin, Jiangsu, China, as seamless rolled rings, forged rings, flanges, round bars, shafts, discs, tube sheets, sleeves, bushings, bored cylinders and valve parts.

Source page: https://www.steelforgepieces.com/Stainless-Steel/UNS-S31635.html
Revision: 2026-10-07

## Grade identification

| Field | Value |
|---|---|
| UNS | S31635 |
| EN number | 1.4571 |
| EN name | X6CrNiMoTi17-12-2 |
| AISI and ASTM type | 316Ti |
| ASME | SA-240 Grade 316Ti |
| JIS | SUS 316Ti |
| AFNOR | Z6 CNDT 17-12 |
| BS | 320S31 |
| GB, China | 06Cr17Ni12Mo2Ti |
| GOST | 08Ch17N13M2T, 10Ch17N13M2T |
| PN | H17N13M2T |
| CSN and STN | 17 348 |
| Structure | Austenitic, non-magnetic as annealed |
| PREN | 24 to 26 |

The designations describe the same material but are not numerically interchangeable. The EN grade runs a narrower molybdenum band and a tighter sulphur limit than the ASTM grade.

## Chemical composition, percent by mass

| Element | ASTM A240 and ASME SA-240 Type 316Ti | EN 1.4571 |
|---|---|---|
| Carbon, C | 0.08 max | 0.08 max |
| Manganese, Mn | 2.0 max | 2.0 max |
| Silicon, Si | 0.75 max | 1.0 max |
| Phosphorus, P | 0.045 max | 0.045 max |
| Sulphur, S | 0.030 max | 0.015 max |
| Chromium, Cr | 16.0 to 18.0 | 16.5 to 18.5 |
| Nickel, Ni | 10.0 to 14.0 | 10.5 to 13.5 |
| Molybdenum, Mo | 2.0 to 3.0 | 2.0 to 2.5 |
| Nitrogen, N | 0.10 max | not specified |
| Titanium, Ti | 5 x (C+N) min, 0.70 max | 0.70 max |
| Iron, Fe | Balance | Balance |

Titanium is the defining element. ASTM sets it at a minimum of five times the combined carbon and nitrogen content with a 0.70 percent ceiling, which guarantees the carbon is tied up rather than free to form chromium carbides.

## Mechanical and physical properties, solution annealed

| Property | At 20 C | At 600 C |
|---|---|---|
| Tensile strength | 515 MPa / 75 ksi min | 380 MPa / 55 ksi min |
| Yield strength, 0.2 percent proof | 205 MPa / 30 ksi min | 160 MPa / 23 ksi min |
| Elongation | 40 percent min | 35 percent min |
| Reduction of area | 50 percent min | not specified |
| Hardness | 217 HB max | not specified |
| Modulus of elasticity | 193 GPa | 165 GPa |
| Thermal conductivity | 14.6 W/m.K | not specified |
| Coefficient of thermal expansion | 16.5 x 10-6 per C | not specified |

### Allowable stress, ASME Section II Part D Table 1A

| Temperature | 100 C | 300 C | 500 C | 600 C | 700 C |
|---|---|---|---|---|---|
| MPa | 138 | 115 | 96 | 85 | 65 |
| ksi | 20.0 | 16.7 | 13.9 | 12.3 | 9.4 |

Use the code table of the governing edition for design.

## Corrosion behaviour

Molybdenum at 2 to 3 percent gives the same pitting and crevice resistance as 316 and 316L, with a PREN of 24 to 26 and a critical pitting temperature around 30 C by ASTM G48. Practical service extends to roughly 2,000 ppm chloride. Titanium adds what the plain grades lack: the weld zone and heat-affected zone stay resistant to intergranular attack, and material passes ASTM A262 Practice E even after an hour at 700 C.

The grade was developed in the 1960s to address polythionic acid stress corrosion cracking in refineries and sensitisation in welded 316. It resists atmospheric and mild corrosion better than the 18Cr-8Ni grades and is more resistant than other chromium-nickel types to sulphuric acid solutions.

Limits: titanium stabilisation does not give immunity to chloride stress corrosion cracking, so hot chloride duty needs assessment against duplex or super-austenitic alternatives.

## Heat treatment, welding and machining

- **Annealing.** 1010 to 1120 C, cooled rapidly in air or water. Best corrosion resistance when the final annealing temperature is above 1070 C.
- **Stress relieving.** 200 to 400 C, air cool.
- **Hardening.** Not possible by heat treatment. Strength is raised only by cold work.
- **Sensitisation range.** 450 to 850 C.
- **Welding.** ER316Ti or ER316L filler by GTAW or SMAW at 1.0 to 1.5 kJ/mm heat input. No preheat and no post-weld anneal for most joints.
- **Machining.** Not a free-machining grade and not recommended for aggressive high-speed machining.
- **Magnetic response.** Non-magnetic as annealed. Cold work induces under about 10 percent martensite and slight magnetism, removed by full annealing.
- **Upper temperature.** ASME Section VIII Division 1 allows SA-240 316Ti to a maximum design temperature of 815 C or 1500 F. Oxidation data gives continuous service to about 870 C and intermittent service to about 925 C.

## Forged shapes and size envelope

| Product | Size limit | Set by |
|---|---|---|
| Seamless rolled rings | up to 6,000 mm outside diameter | 6 m radial-axial ring mill |
| Small and mid-range rings | from 50 mm outside diameter | Upset and punch route, 1 m and 3 m mills |
| Flanges | ASME B16.5, B16.47, API 6A | Press and ring mills |
| Shafts and spindles | up to 14,000 mm turned length | C61160 lathe, 15 m well furnace |
| Discs, tube sheets, blocks | up to 5,000 mm machined diameter | 5,000 mm vertical turning lathe |
| Bored cylinders, sleeves, bushings | up to 1,600 mm dia x 10,000 mm | CNC deep-hole drilling machine |
| Bars, flats and blocks | press capacity | 6,300 t, 4,000 t and 2,000 t presses |
| Single-piece weight | up to 30,000 kg | 60 t heat size, 6,300 t press |

Valve and wellhead parts are a regular order in this grade: bodies, bonnets, blocks, stems, seat rings, spools, nozzles and manifolds, including work to API 6A and NACE MR0175 or ISO 15156.

## Applications

Petrochemical and refining heat exchangers, catalytic recovery systems and recuperators. Power generation boiler and superheater components. Chemical acid reactors, transport containers and process vessels. Pulp and paper digesters, liquor tanks and paper machine parts. Exhaust manifolds, ducting and thermal oxidisers under thermal cycling. Desalination evaporators. Food, beverage, pharmaceutical, laboratory and medical equipment. Oil and gas subsea and deepwater parts, air compressors, power and nitrogen generators.

## 316Ti against 316L, 316 and 321

| Property | 316Ti, S31635 | 316L, S31603 | 316, S31600 | 321, S32100 |
|---|---|---|---|---|
| Type | Austenitic, Mo, Ti-stabilised | Austenitic, Mo, low carbon | Austenitic, Mo | Austenitic, Ti-stabilised |
| Carbon max | 0.08 | 0.03 | 0.08 | 0.08 |
| Chromium | 16.0 to 18.0 | 16.0 to 18.0 | 16.0 to 18.0 | 17.0 to 19.0 |
| Nickel | 10.0 to 14.0 | 10.0 to 14.0 | 10.0 to 14.0 | 9.0 to 12.0 |
| Molybdenum | 2.0 to 3.0 | 2.0 to 3.0 | 2.0 to 3.0 | none |
| Stabiliser | Ti, 5 x (C+N) min | none | none | Ti, 5 x C min |
| PREN | 24 to 26 | 24 to 26 | 24 to 26 | 18 to 20 |
| Yield min, MPa | 205 | 170 | 205 | 205 |

- **316Ti against 316L.** 316Ti holds up under thermal cycling and carries a higher minimum yield, 205 against 170 MPa. 316L suits ambient welded work and polished surfaces.
- **316Ti against 316.** Similar strength. 316Ti is weld-stable without an anneal, which matters on thick sections.
- **316Ti against 321.** Both titanium-stabilised, but 321 has no molybdenum and a PREN of 18 to 20. 316Ti for wet corrosion with heat, 321 for dry high-temperature oxidation.

## Testing and certification

- Ultrasonic testing to EN 10228-3, SEP 1921 or ASTM A388 on PXUT-3300, USM35XS and CTS-22 flaw detectors, to the nominated acceptance class.
- Chemical analysis by optical emission spectrometry to ASTM E415, infrared carbon and sulphur analysis to ASTM E1019, and handheld positive material identification.
- Mechanical testing on 600 kN and 300 kN universal machines to ASTM A370 and ISO 6892. Charpy V-notch impact to minus 60 C in-house.
- Intergranular corrosion testing to ASTM A262 or ASTM G28 and pitting resistance to ASTM G48, placed with an accredited third-party laboratory and reported with the mill certificate.
- Magnetic particle inspection to ASTM E709 and metallographic grain size to ASTM E112 on site.
- Certification to EN 10204 3.1, or EN 10204 3.2 witnessed by BV, DNV, LR, SGS, TUV or the customer's own inspector. Works approvals CCS, BV, DNV, LR, NK.
- Traceability from melt number through forging, heat treatment and machining, all inside one works.

## Supplier

| Field | Detail |
|---|---|
| Legal name | Jiangyin Jiangnan Metal Co., Ltd. |
| Business | Integrated melting works, open-die forge, ring rolling mill |
| Established | 1997 |
| Employees | 460, including 9 senior engineers, 32 intermediate engineers and 140 technicians |
| Works | No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China |
| Melting | EF, LF, VOD, VIM, VAR, ESR. 60 t maximum heat |
| Forging | 6,300 t press, 6 m ring mill, 30 t maximum single piece |
| Approvals | CCS, BV, DNV, LR, NK |
| Minimum order | 10 kg, no minimum piece count |
| Lead time | 20 to 60 days |
| Business hours | Monday to Saturday, 08:00 to 17:30 China Standard Time, UTC+8 |
| Telephone | +86 189 2135 9659 |
| Email | sales@steelforgepieces.com |
| Website | https://www.steelforgepieces.com/ |

## Frequently asked questions

### What is UNS S31635?

A titanium-stabilised, molybdenum-bearing austenitic stainless steel of nominal 16Cr-12Ni-2Mo-Ti composition, designated 316Ti and EN 1.4571. Titanium at a minimum of five times the combined carbon and nitrogen content stops chromium carbide precipitation during welding or exposure between 450 and 850 C.

### Is UNS S31635 the same as 316Ti and 1.4571?

Same material, different limits. ASTM allows Cr 16.0 to 18.0, Ni 10.0 to 14.0, Mo 2.0 to 3.0, S 0.030 max. EN 1.4571 specifies Cr 16.5 to 18.5, Ni 10.5 to 13.5, Mo 2.0 to 2.5, S 0.015 max.

### What is the chemical composition?

To ASTM A240 and ASME SA-240: C 0.08 max, Mn 2.0 max, Si 0.75 max, P 0.045 max, S 0.030 max, Cr 16.0 to 18.0, Ni 10.0 to 14.0, Mo 2.0 to 3.0, N 0.10 max, Ti 5 x (C+N) min to 0.70 max, balance iron.

### What are the mechanical properties?

Solution annealed at room temperature: tensile 515 MPa minimum, 0.2 percent proof stress 205 MPa minimum, elongation 40 percent minimum, reduction of area 50 percent minimum, hardness 217 HB maximum, modulus 193 GPa. At 600 C: 380 MPa tensile, 160 MPa yield, 35 percent elongation.

### How is it heat treated after forging?

Anneal 1010 to 1120 C with a rapid cool in air or water, above 1070 C for best corrosion resistance. Stress relieve 200 to 400 C, air cool. Not hardenable by heat treatment.

### Does it need post-weld heat treatment?

No. Titanium holds carbon and nitrogen as Ti(C,N), so the weld zone keeps its corrosion resistance. Use ER316Ti or ER316L filler at low heat input, around 1.0 to 1.5 kJ/mm.

### 316Ti or 316L?

316Ti where the part is thermally cycled or held between 450 and 850 C, and where the higher minimum yield of 205 MPa helps. 316L for ambient welded work and polished surfaces.

### What is the maximum service temperature?

ASME Section VIII Division 1 allows SA-240 316Ti to a maximum design temperature of 815 C or 1500 F. Oxidation data gives continuous service to about 870 C and intermittent to about 925 C.

### Is it magnetic?

Non-magnetic as annealed. Cold work induces slight magnetism, removed by full annealing.

### Is it suitable for seawater?

PREN 24 to 26 and a critical pitting temperature around 30 C, with titanium keeping weld zones resistant, which is why the grade appears in desalination evaporators and offshore heat exchangers. Not immune to chloride stress corrosion cracking, so hot chloride duty needs assessment.

### What is the minimum order and lead time?

10 kg minimum with no minimum piece count. Lead time 20 to 60 days.

### Which forged shapes are available in this grade?

Seamless rolled rings to 6,000 mm outside diameter, forged rings from 50 mm, flanges to ASME B16.5, B16.47 and API 6A, shafts to 14,000 mm turned length, discs and tube sheets to 5,000 mm machined diameter, bored cylinders and sleeves to 1,600 mm diameter by 10,000 mm, bars, blocks and valve parts, to a 30 tonne maximum single piece.

---

Data compiled from ASTM A240 and ASME SA-240 for Type 316Ti, ASTM A276 and A479 for bar, EN 10088-2, EN 10088-3 and EN 10028-7 for 1.4571, and ASME Section II Part D Table 1A. Given for guidance and not a substitute for the governing specification.
