# UNS S31000 Forgings: Type 310 / ASTM A182 F310

**UNS S31000 is Type 310 heat-resistant austenitic stainless steel, nominally 25 per cent chromium and 20 per cent nickel, with carbon up to 0.25 per cent. As a forging it is normally ordered to ASTM A182 grade F310. Jiangyin Jiangnan Metal Co., Ltd. melts this grade in its own furnaces in Jiangyin, Jiangsu, China, then forges, ring-rolls, heat-treats, machines and tests it on the same site.**

The chromium and silicon give oxidation resistance to 1050 C in continuous service, resistance to sulphidation, and usable life in moderately carburising atmospheres. The fully austenitic structure stays tough down to -268 C and keeps low magnetic permeability, which is why the grade also appears in cryogenic work.

| Field | Detail |
|---|---|
| UNS number | S31000 |
| AISI type | 310 |
| Werkstoff number | 1.4845 |
| Forging specification | ASTM A182 grade F310 |
| Chromium | 24.0 to 26.0 per cent |
| Nickel | 19.0 to 22.0 per cent |
| Carbon | 0.25 per cent maximum |
| Molybdenum | None specified |
| Density | 7.89 g/cm3 |
| Maximum continuous service | 1050 C in oxidising conditions, sulphur up to 2 g/m3 |
| Minimum service | -268 C |
| Solution anneal | 1100 to 1150 C followed by rapid quench |
| Supplier | Jiangyin Jiangnan Metal Co., Ltd., No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China |
| Telephone | +86 189 2135 9659 |
| Email | sales@steelforgepieces.com |
| Page | https://www.steelforgepieces.com/Stainless-Steel/UNS-S31000.html |

## 310, 310S and 310H are three different UNS numbers

All three share the same 25Cr 20Ni base and differ in carbon. They are not interchangeable on a certificate. Writing S31000 and 310H on the same line of an enquiry is the most common ordering error on this grade, because carbon raises creep strength and lowers corrosion resistance after welding.

| Grade | UNS | Carbon | Silicon | Why it is chosen |
|---|---|---|---|---|
| 310 | S31000 | 0.25 max | 1.50 max | General heat-resisting workhorse |
| 310S | S31008 | 0.08 max | 1.50 max | Low carbon, easier fabrication and welding |
| 310H | S31009 | 0.04 to 0.10 | 0.75 max | Carbon held high and narrow for creep resistance |

If a drawing says 310H, we melt to S31009 limits and the grain size requirement changes with it. The UNS number has to be confirmed before the heat is cast.

## Chemical composition

For forged pressure parts the governing chemistry is ASTM A182 grade F310, listed in that specification as the 25 chromium 20 nickel alloy. Silicon is the column that catches people out: A182 forgings are held to 1.00 per cent maximum, while Type 310 plate to ASTM A240 is allowed 1.50 per cent. Typical silicon sits near 0.6 per cent.

| Limit | C | Mn | Si | P | S | Cr | Ni | Mo | Fe |
|---|---|---|---|---|---|---|---|---|---|
| Minimum | - | - | - | - | - | 24.00 | 19.00 | - | Balance |
| Maximum | 0.25 | 2.00 | 1.00 | 0.045 | 0.030 | 26.00 | 22.00 | Not specified | Balance |

There is no deliberate molybdenum addition, and that single fact decides most of what this grade should and should not be used for.

## Mechanical properties

Design to the A182 acceptance minimum, expect the typical annealed value.

| Property | ASTM A182 F310 minimum | Typical, solution annealed |
|---|---|---|
| Tensile strength | 515 MPa (75 ksi) | 550 MPa (80 ksi) |
| Yield strength, 0.2 per cent offset | 205 MPa (30 ksi) | 245 MPa (35 ksi) |
| Elongation in 2 in. or 4D | 30 per cent | 45 per cent |
| Reduction of area | 50 per cent | Not quoted |
| Hardness | Not mandated for austenitic grades in A182 | 217 HB maximum |

### Creep

Most S31000 forgings work hot, so creep rather than room temperature tensile strength usually sets the section. All values MPa.

| Temperature | Creep strain 1 000 h | 10 000 h | 100 000 h | Creep rupture 1 000 h | 10 000 h | 100 000 h |
|---|---|---|---|---|---|---|
| 600 C | 120 | 100 | 40 | 200 | 140 | 80 |
| 700 C | 50 | 35 | 20 | 80 | 45 | 20 |
| 800 C | 20 | 10 | 8 | 35 | 20 | 8 |
| 900 C | 10 | 6 | 3 | 15 | 10 | 5 |
| 1000 C | 5 | 3 | 1.5 | 9 | 4 | 2 |

### Physical properties

| Property | Metric | Imperial |
|---|---|---|
| Density | 7.89 g/cm3 | 0.285 lb/in3 |
| Modulus of elasticity | 196 GPa | 28.5 x 10^6 psi |
| Melting range | 1354 to 1402 C | 2470 to 2555 F |
| Specific heat, 0 to 100 C | 502 J/kg-K | 0.12 BTU/lb-F |
| Thermal conductivity | 10.8 W/m-K | 8.0 BTU/hr/ft2/ft/F |
| Electrical resistivity at 20 C | 78.0 microhm-cm | 30.7 microhm-in |

## Service temperature by atmosphere

The oxidation limit is not one number. It moves with the sulphur load and the oxygen potential of the gas.

| Atmosphere | Limit |
|---|---|
| Oxidising, sulphur up to 2 g/m3 | 1050 C continuous, 1100 C peak |
| Oxidising, sulphur above 2 g/m3 | 950 C maximum |
| Low oxygen, sulphur up to 2 g/m3 | 1000 C maximum |
| Nitriding or carburising | 850 to 950 C maximum |
| Cryogenic | Tough to -268 C, low magnetic permeability |

In reducing, nitriding and carburising gas the alloy does not match Alloy 600 or Alloy 800, but it outperforms most heat-resisting stainless steels in those conditions.

## Applications

- **Thermal processing.** Annealing covers and boxes, muffles and retorts, burner grids, doors, fans, walking beams, recuperators.
- **Furnace parts.** Burners, doors, fans, piping, recuperators, heat-treatment baskets and jigs.
- **Fluidised bed furnaces.** Coal combustor internals, grids, piping, wind boxes.
- **Petroleum refining.** Catalytic recovery system parts, flares, recuperators, tube hangers.
- **Power generation.** Coal gasifier internals, pulverised coal burners, tube hangers.
- **Sintering and cement plant.** Burners, burner shields, feeding and discharging systems, wind boxes.
- **Ore processing and steel plant.** Smelter and steel melting equipment, continuous casting equipment.
- **Cryogenic components.** Where toughness to -268 C and low magnetic permeability are required.
- **Food processing.** Equipment and storage exposed to high temperature cleaning cycles.

## Product forms and size envelope

| Family | Items | Envelope |
|---|---|---|
| Rings | Seamless rolled rings, forged rings, retaining rings, valve seat rings, gear ring blanks | OD 50 to 6000 mm |
| Flanges and flat work | Weld neck, blind, slip-on, socket weld and orifice flanges, tube sheets, covers, blocks | To 5000 mm machined diameter |
| Shafts and bars | Round, flat and square bars, stepped shafts, eccentric shafts, spindles, gear shafts | To 14 000 mm turned length |
| Hollow sections | Cylinders, sleeves, bushings, couplings, heavy-wall pipe bored from solid | To 1600 mm dia x 10 000 mm bored |
| Discs and wheels | Forged discs, blanks, hubs, wheels, rolls | To 30 t single piece |
| Valve and vessel parts | Bodies, bonnets, stems, seat rings, nozzles, manifolds | Forged from one piece, no welds |

Minimum order is 10 kg with no minimum piece count. Normal lead time is 20 to 60 days.

## Where this grade is the wrong choice

- **Wet or chloride corrosion.** Alloy 310 is not designed for service in wet corrosive environments. The high carbon that gives creep strength is detrimental to aqueous corrosion resistance, and the alloy is prone to intergranular corrosion after long exposure at high temperature. With no molybdenum, chloride pitting and crevice resistance is weak. Use ASTM A182 F44, duplex F51, F53 or F55, 904L or Incoloy 825 for seawater, desalination, subsea or sour duty.
- **Sigma phase.** Between 650 and 950 C the alloy precipitates sigma phase and loses toughness. A solution anneal at 1100 to 1150 C restores a degree of it.
- **Severe carburising.** The harsher carburising atmospheres in thermal process plant normally need a nickel alloy such as Alloy 330, Inconel 600 or Incoloy 800H.
- **Cold forming before hot service.** The alloy forms much like 316, but cold forming parts destined for long term high temperature exposure is not recommended because of carbide and sigma phase precipitation.
- **Creep-critical duty.** Specify 310H (S31009) with its controlled carbon rather than S31000.

## Manufacturing route

**Melting.** Stainless grades run through the 25 t electric arc furnace, are refined in a 25 t or 50 t ladle furnace, and are decarburised under vacuum in the 30 t or 60 t VOD units. Protective-atmosphere electroslag remelting at 3 t or 6 t is available where cleanliness governs. Maximum heat size is 60 tonnes. Because the melt is on site, the certificate traces a part back to its melt number rather than stopping at a purchased billet.

**Forging.** Hot working between 950 and 1200 C on 6300 t, 4000 t and 2000 t hydraulic presses, with radial-axial ring mills at 6 m, 3 m and 1 m, backed by hammers from 750 kg to 5 t.

**Heat treatment.** Final anneal at 1000 to 1150 C followed by rapid quenching after hot forming. Fourteen furnaces on site, including two 15 m deep well-type furnaces that allow long shafts to be quenched vertically.

## Testing and certification

| Item | Method or standard |
|---|---|
| Chemical analysis | Optical emission spectrometry to ASTM E415, infrared carbon and sulphur to ASTM E1019, handheld PMI |
| Tensile and elongation | ASTM A370 or ISO 6892, acceptance to A182 F310 |
| Ultrasonic testing | ASTM A388 or SEP 1921. In European practice the part covering austenitic forgings is EN 10228-4, not EN 10228-3 |
| Surface | Liquid penetrant. Magnetic particle does not apply to this austenitic grade |
| Grain size | ASTM E112 metallography on site |
| Intergranular corrosion | ASTM A262 or ASTM G28, placed with an accredited third-party laboratory |
| Certification | EN 10204 3.1 as standard, EN 10204 3.2 witnessed by BV, DNV, LR, SGS, TUV or the customer's inspector on request |
| Class approvals | CCS, BV, DNV, LR, NK |

## Designations

| System | Designation |
|---|---|
| UNS | S31000 |
| AISI type | 310 |
| Werkstoff | 1.4845 |
| Forgings | ASTM A182 grade F310 |
| Plate and flat product | ASTM A240, ASME SA240, AMS 5521 |
| Related grades | S31008 (310S), S31009 (310H) |

## Requesting a quotation

Send the grade, the dimensions or a drawing, the quantity, the delivery condition, the heat treatment and testing requirements, and the destination port. Six items in the first email usually gets a price back within two working days.

| # | Item | Example |
|---|---|---|
| 1 | Grade or specification | UNS S31000 / ASTM A182 F310 |
| 2 | Dimensions or drawing (PDF, DWG, DXF, STEP) | OD 1400 x ID 1100 x H 240 mm |
| 3 | Quantity and repeat volume | 8 pcs, about three times a year |
| 4 | Delivery condition | As-forged, proof-machined or finish-machined |
| 5 | Heat treatment and testing | Solution annealed, UT to ASTM A388, ASTM A262 Practice E |
| 6 | Certification and destination port | EN 10204 3.2 witnessed by DNV, Rotterdam |

## Frequently asked questions

### Is UNS S31000 the same as 310H?

No. UNS S31000 is Type 310, carbon 0.25 per cent maximum. 310H is UNS S31009, carbon held between 0.04 and 0.10 per cent for enhanced creep resistance. 310S is the low carbon version, UNS S31008, at 0.08 per cent maximum. Silicon differs too: 1.50 per cent for 310 and 310S against 0.75 per cent for 310H. Jiangyin Jiangnan Metal forges all three, but the UNS number has to be stated on the enquiry because the chemistry is fixed before the ingot is cast.

### What is the chemical composition of UNS S31000 forgings?

To ASTM A182 grade F310: carbon 0.25 per cent maximum, manganese 2.00 per cent maximum, silicon 1.00 per cent maximum, phosphorus 0.045 per cent maximum, sulphur 0.030 per cent maximum, chromium 24.00 to 26.00 per cent, nickel 19.00 to 22.00 per cent, balance iron. The silicon limit is the one that catches people out: A182 forgings are held to 1.00 per cent maximum while Type 310 plate to ASTM A240 is allowed 1.50 per cent.

### What is the maximum service temperature of UNS S31000?

In oxidising conditions with sulphur up to 2 g/m3, 1050 C continuous with a 1100 C peak. Above 2 g/m3 sulphur the ceiling falls to 950 C. In a low oxygen atmosphere it is 1000 C, and in nitriding or carburising gas 850 to 950 C. At the cold end the alloy stays tough to -268 C with low magnetic permeability.

### Can UNS S31000 be used in seawater or wet chloride service?

No. Alloy 310 is not designed for service in wet corrosive environments. The high carbon content that gives it creep strength has a detrimental effect on aqueous corrosion resistance, and the alloy is prone to intergranular corrosion after long term exposure at high temperature. There is no molybdenum, so chloride pitting resistance is weak. Jiangyin Jiangnan Metal supplies ASTM A182 F44, duplex F51, F53 and F55, 904L or Incoloy 825 for those duties.

### Which ultrasonic testing standard applies to UNS S31000 forgings?

Type 310 is fully austenitic, so in European practice the applicable part is EN 10228-4, covering ultrasonic testing of austenitic and austenitic-ferritic stainless steel forgings. EN 10228-3 is written for ferritic and martensitic forgings and is not the right part for this grade. ASTM A388 or SEP 1921 can be used instead.

### What size and weight of UNS S31000 forgings can you make?

Seamless rings roll to 6000 mm outside diameter on the 6 m radial-axial mill, with 3 m and 1 m mills below that and an upset-and-punch route for rings from 50 mm outside diameter. The heaviest single forging is 30 tonnes. Shafts turn to 14 m between centres and bores run to 1600 mm diameter by 10 000 mm deep. Minimum order is 10 kg with no minimum piece count.

### Do you melt UNS S31000 in house or buy billet?

It is melted on site, through the 25 t electric arc furnace, 25 t and 50 t ladle furnaces and 30 t or 60 t VOD units, with electroslag remelting available where cleanliness governs. Maximum heat size is 60 tonnes. The certificate traces a part back to its melt number rather than stopping at a purchased billet certificate.

### Is UNS S31000 weldable?

Yes, by TIG, plasma, MIG, SMAW, SAW and FCAW. Where corrosion resistance after welding matters, the low carbon 310S version is the better choice because it limits carbide precipitation in the heat affected zone.

### What is the lead time?

20 to 60 days from order confirmation. Standard stainless grades melted through the arc furnace sit at the lower end. Anything needing a remelting step, third-party witnessed inspection or outside laboratory corrosion testing sits at the upper end.

---

Jiangyin Jiangnan Metal Co., Ltd. No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China. Telephone, WhatsApp and WeChat +86 189 2135 9659. Email sales@steelforgepieces.com. Business hours Monday to Saturday, 08:00 to 17:30 China Standard Time (UTC+8).

Last reviewed 5 October 2026. Composition and mechanical minima are quoted from ASTM A182 grade F310. Physical, creep and service temperature figures are representative published values for alloy 310, given for guidance and not as a warranty of fitness for a particular application.