# UNS S13800 (PH13-8Mo) Open-Die Forgings

**UNS S13800 is a martensitic precipitation hardening stainless steel containing 12.25 to 13.25 % chromium, 7.50 to 8.50 % nickel, 2.00 to 2.50 % molybdenum and 0.90 to 1.35 % aluminium. It combines high strength and hardness with high toughness and good resistance to stress-corrosion cracking, and shows little difference between longitudinal and transverse properties. Jiangyin Jiangnan Metal Co., Ltd. melts this grade on site and forges it in the same works.**

The alloy is also known as PH 13-8 Mo, 13-8 PH, alloy 13-8, ASTM grade XM-13, EN 1.4534 and X3CrNiMoAl13-8-2. PH 13-8 Mo is a registered trademark of Armco Inc.

Source page: https://www.steelforgepieces.com/Stainless-Steel/UNS-S13800.html

## Grade record

| Field | Detail |
|---|---|
| UNS number | S13800 |
| ASTM and ASME grade | XM-13 |
| EN material number | 1.4534 |
| EN steel name | X3CrNiMoAl13-8-2 |
| Forgings | ASTM A705 / ASME SA705 |
| Bar, wire, shapes | ASTM A564 / ASME SA564 Grade XM13 |
| Bar, wire, forgings, rings, extrusions | AMS 5629, Type 1 |
| Sheet, strip, plate | ASTM A693 / ASME SA693, AMS 5864 |
| Conditions supplied | A, H950, H1000, H1025, H1050, H1100, H1150, H1150M, RH950 |
| Melt routes available | VIM + VAR, ESR, EAF + LF + VOD |
| Maximum single piece | 30,000 kg |
| Minimum order | 10 kg, no minimum piece count |
| Lead time | 20 to 60 days |
| Supplier | Jiangyin Jiangnan Metal Co., Ltd., No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China |
| Telephone | +86 189 2135 9659 |
| Email | sales@steelforgepieces.com |

Note on specifications: ASTM B564 is sometimes written on enquiries for this grade. B564 covers nickel-alloy forgings and does not list UNS S13800. For a stainless precipitation hardening forging the correct reference is ASTM A705 Grade XM-13, or AMS 5629 for aerospace work.

## Chemical composition

Weight percent, UNS S13800 type analysis.

| Limit | C | Si | Mn | P | S | Cr | Mo | Ni | Al | N | Fe |
|---|---|---|---|---|---|---|---|---|---|---|---|
| Min | - | - | - | - | - | 12.25 | 2.00 | 7.50 | 0.90 | - | Bal. |
| Max | 0.05 | 0.10 | 0.10 | 0.010 | 0.008 | 13.25 | 2.50 | 8.50 | 1.35 | 0.010 | - |

Silicon and manganese are held to 0.10 %, phosphorus to 0.010 %, sulphur to 0.008 % and nitrogen to 0.010 %. Properties depend on meeting those limits and on a melt practice that controls impurities and segregation. Aluminium is the hardening element.

## Melting

Material to AMS 5629 is normally double melted: vacuum induction melting followed by consumable-electrode vacuum arc remelting. This works runs a 3 t vacuum induction furnace, a 6 t vacuum arc remelting furnace and 3 t and 6 t protective-atmosphere electroslag furnaces, so double-melted ingot is produced on site rather than subcontracted. Where a remelted ingot is not required, the electric arc furnace, ladle furnace and vacuum oxygen decarburisation route is used, with a 60 t maximum heat.

## Mechanical properties

Specified room-temperature minima, longitudinal direction, AMS 5629 and ASTM A564 Grade XM13 basis.

| Condition | 0.2 % proof stress | Tensile strength | Elongation | Reduction of area | Hardness |
|---|---|---|---|---|---|
| A, solution treated | not specified | not specified | - | - | 363 HB max |
| H950 | 1413 MPa / 205 ksi | 1517 MPa / 220 ksi | 10 % | 45 % | 45 HRC |
| H1000 | 1310 MPa / 190 ksi | 1413 MPa / 205 ksi | 10 % | 50 % | 43 HRC |
| H1025 | 1207 MPa / 175 ksi | 1276 MPa / 185 ksi | 11 % | 50 % | 41 HRC |
| H1050 | 1138 MPa / 165 ksi | 1207 MPa / 175 ksi | 12 % | 50 % | 40 HRC |
| H1100 | 931 MPa / 135 ksi | 1034 MPa / 150 ksi | 14 % | 50 % | 34 HRC |
| H1150 | 621 MPa / 90 ksi | 931 MPa / 135 ksi | 14 % | 50 % | 30 HRC |

Published typical values sit above these minima. Typical longitudinal H1000 properties run near 1413 MPa proof stress and 1482 MPa tensile strength at 13 % elongation and 45 HRC. Charpy V-notch impact energy rises with ageing temperature, from about 27 J in H950 to about 103 J in H1150 and about 163 J in the overaged H1150M condition. Transverse typical values stay close to longitudinal, which is why the grade is specified for thick forged sections.

## Physical properties

| Property | Value |
|---|---|
| Density, H1000 | 7.76 g/cm3, 0.280 lb/in3 |
| Modulus of elasticity, H1000 | 195 GPa, 28.3 x 10^3 ksi |
| Thermal conductivity at 100 C | 14.0 W/m.K |
| Mean thermal expansion, 21 to 316 C | 11.2 x 10^-6 /K |
| Magnetic response | Ferromagnetic in all conditions |
| Oxidation resistance | Good to about 593 C (1100 F) |

## Forging

Stock is heated uniformly to 1175 to 1205 C (2150 to 2200 F) and held about one hour at temperature. Forging stops above 955 C (1750 F). The forging is air cooled to about 16 C (60 F), which sets the grain size. Every hot-worked piece is solution treated before ageing, otherwise it will not respond correctly to the ageing treatment.

## Heat treatment

Ageing is four hours at temperature followed by air cooling.

| Condition | Treatment | Notes |
|---|---|---|
| A | 925 C +/- 8 C, cool below 16 C | Solution treated, fully martensitic. Sections under about 230 cm2 may be liquid quenched, heavier sections air cooled |
| H950 | 510 C, 4 h, air cool | Highest strength and hardness, slowest machining |
| H1000 | 538 C, 4 h, air cool | Lowest ageing temperature suggested where stress-corrosion cracking governs |
| H1025 | 552 C, 4 h, air cool | Balance of strength and toughness |
| H1050 | 566 C, 4 h, air cool | Common on valve and pump parts |
| H1100 | 593 C, 4 h, air cool | Higher toughness, easier machining |
| H1150 | 621 C, 4 h, air cool | Overaged, needs re-solution treatment before further ageing |
| RH950 | Cold treat to -73 C for 2 h within 24 h of solution treatment, warm to room temperature, then 510 C, 4 h, air cool | Highest typical strength level |
| H1150M | 760 C, 2 h, air cool, then 621 C, 4 h, air cool | Best machinability, needs re-solution treatment for higher strengths |

Ageing contracts the part by a predictable amount: about 0.0004 to 0.0006 in/in for H950 and H1000, 0.0005 to 0.0008 for H1050, and 0.0008 to 0.0012 for H1100. The hardness range of H1150 overlaps the solution-treated range, so a hardness reading alone cannot identify the condition. The heat treatment record on the certificate is the evidence.

## Machining, welding and corrosion

In condition A the grade machines with good tool life at surface speeds roughly 20 to 30 % below those used on 17Cr-4Ni and on Types 302 and 304. Machinability in the aged conditions improves as the ageing temperature rises, and H1150M is the easiest. At 45 HRC minimum, H950 machining is slow and hard on tooling, so the usual sequence is rough machine in condition A, age, then finish. Bar and forging stock is cold sawn, not abrasive cut, because abrasive wheel cutting can leave fine surface cracks.

Welding runs by inert-gas shielded or resistance processes, with matching 13-8 filler where the weld must match the base metal and an austenitic filler such as E/ER308L where it need not. Welding in the solution-annealed condition is normally satisfactory. The best combination of strength, ductility and corrosion resistance comes from solution treating the welded part and then ageing it.

In the H950 condition, resistance to rusting in 5 % salt fog is similar to Type 304, and general resistance in strongly oxidising and reducing acids and in atmospheric exposure approaches Type 304. Corrosion resistance is highest fully hardened and falls slightly as ageing temperature rises, while resistance to stress-corrosion cracking improves with ageing temperature. Finished parts are supplied free of scale and embedded iron, and passivated.

## Forged forms supplied in UNS S13800

Forged rings and seamless rolled rings, forged flanges, forged round bars and billets, forged shafts, spindles and eccentric shafts, forged discs, tube sheets and covers, forged sleeves, bushings and bored cylinders, and valve parts including bodies, bonnets, stems, seat rings and blocks.

| Product | Size limit |
|---|---|
| Seamless rolled rings | up to OD 6,000 mm, from OD 50 mm by upsetting and punching |
| Forged shafts | up to 14,000 mm turned length |
| Discs, tube sheets, blocks | up to 5,000 mm machined diameter |
| Bored cylinders and hollow shafts | up to 1,600 mm dia x 10,000 mm |
| Single-piece weight | up to 30,000 kg |

## Applications

Published applications for the alloy are valve parts and fittings, cold-headed and machined fasteners, shafts and pins, landing gear components, lockwashers, aerospace parts, nuclear reactor components, injection moulding equipment, and petrochemical duty requiring resistance to stress-corrosion cracking. Most of our own output in this grade goes out as valve stems, seat rings and bodies for ball, gate, globe and check valves, as pump and compressor shafts and sleeves, and as forged rings and discs for rotating equipment.

For large pressure-boundary components, 17-4 PH and 15-5 PH are worth pricing alongside this grade, because 13-8 costs more and its extra toughness is not always being used.

## Inspection and certification

Ultrasonic examination to EN 10228-3, SEP 1921 or ASTM A388, to the acceptance class on the purchase order. Chemical analysis, tensile test, hardness and, where required, Charpy V-notch impact test are reported on an inspection certificate to EN 10204 type 3.1, or type 3.2 counter-signed by a third party such as SGS, BV, TUV or Lloyd's Register. Dimensional reports, positive material identification, liquid penetrant examination, grain size and intergranular corrosion testing on request. Heat-number traceability runs from melt to shipped part. The works holds CCS, BV, DNV, LR and NK approvals.

## Questions

**Is UNS S13800 the same as PH13-8Mo?**
Yes. UNS S13800 is the unified numbering designation for the alloy sold as PH 13-8 Mo, also called 13-8 PH, alloy 13-8, XM-13, 1.4534 and X3CrNiMoAl13-8-2.

**Which specification goes on a forging order?**
ASTM A705 or ASME SA705, grade XM-13, with the condition required. Bar and machined-from-bar parts go to ASTM A564 Grade XM13, aerospace work to AMS 5629.

**What are the H950 properties?**
Minimum 1413 MPa (205 ksi) proof stress, 1517 MPa (220 ksi) tensile strength, 10 % elongation, 45 % reduction of area, 45 HRC.

**At what temperature is the grade forged?**
Heat to 1175 to 1205 C, hold about one hour, finish above 955 C, air cool to about 16 C, then solution treat before ageing.

**Which aged condition should be specified?**
H950 for maximum strength. H1000 and above for higher toughness and better resistance to stress-corrosion cracking, with 538 C the suggested minimum where cracking governs. H1150 and H1150M are overaged conditions for easier machining and need re-solution treatment before further ageing.

**Can double-melted material to AMS 5629 be supplied?**
Yes. Vacuum induction melting at 3 t, vacuum arc remelting at 6 t, and protective-atmosphere electroslag at 3 t and 6 t run in this works.

**Is UNS S13800 magnetic?**
Yes, ferromagnetic in both the solution-treated and aged conditions.

## Requesting a quotation

Send a drawing as PDF, DWG or STEP, or the finished dimensions, with the grade and specification (for example UNS S13800 forged ring to ASTM A705 condition H1050), the quantity, the delivery condition, the melt route if specified, the testing and certificate requirements, and the destination port.

Email sales@steelforgepieces.com or telephone +86 189 2135 9659.

## Data basis

Composition, property, forging and heat treatment data follow the published requirements of AMS 5629, ASTM A564 and ASME SA564 Grade XM13, ASTM A705 and ASME SA705, together with mill and distributor data sheets for alloy 13-8. Figures are for design and enquiry work. The governing values for any order are those of the specification and revision written on the purchase order, as reported on the EN 10204 certificate.