# SUS 317 Forgings (AISI 317 / UNS S31700 / EN 1.4449)

**SUS 317 is a molybdenum-bearing austenitic stainless steel, in effect a higher chromium, nickel and molybdenum version of 316.** It contains 18.0 to 20.0 % chromium, 11.0 to 15.0 % nickel and 3.0 to 4.0 % molybdenum, with carbon held to 0.08 % maximum. The extra molybdenum raises strength and improves resistance to pitting and crevice attack in chloride-bearing, moderately oxidising and reducing media, so 317 is specified where 316 is marginal.

Jiangyin Jiangnan Metal Co., Ltd. forges this grade to drawing. Steel is melted on site, forged or ring-rolled, solution annealed, machined and tested without leaving the plant, so the certificate traces back to a melt number rather than a purchased billet.

| Field | Detail |
|---|---|
| Grade | SUS 317 / AISI 317 |
| UNS | S31700 |
| EN number | 1.4449 |
| Forging specification | ASTM A182 / ASME SA182 Grade F317 |
| Structure | Austenitic |
| Low-carbon variant | 317L, UNS S31703 |
| Maximum ring outside diameter | 6,000 mm |
| Maximum single piece | 30 t |
| Minimum order | 10 kg, no minimum piece count |
| Lead time | 20 to 60 days |
| Certification | EN 10204 3.1, or 3.2 witnessed |
| Manufacturer | Jiangyin Jiangnan Metal Co., Ltd. |
| Plant | No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China 214423 |
| Telephone | +86 189 2135 9659 |
| Email | sales@steelforgepieces.com |
| Page | https://www.steelforgepieces.com/Stainless-Steel/SUS-317.html |

## Chemical composition

Limits are the ASTM A182 Grade F317 forging requirement, weight percent.

| Element | Symbol | Specified | Nominal |
|---|---|---|---|
| Carbon | C | 0.08 max | - |
| Chromium | Cr | 18.0-20.0 | 19 |
| Nickel | Ni | 11.0-15.0 | 13 |
| Molybdenum | Mo | 3.0-4.0 | 3.5 |
| Manganese | Mn | 2.00 max | - |
| Silicon | Si | 1.00 max | - |
| Phosphorus | P | 0.045 max | - |
| Sulphur | S | 0.030 max | - |
| Iron | Fe | Balance | 61 |

Chemistry is read at the furnace on a mobile optical emission spectrometer and confirmed on the finished part with a handheld analyser.

## Mechanical properties

Two sets of numbers, and they are not interchangeable. The first is what a forging must achieve on test to be certified. The second is what annealed material typically measures.

### Specified minimums, ASTM A182 F317

| Property | Metric | Imperial |
|---|---|---|
| Tensile strength, min | 515 MPa | 75 ksi |
| Yield strength 0.2 % offset, min | 205 MPa | 30 ksi |
| Elongation in 50 mm or 4D, min | 30 % | 30 % |
| Reduction of area, min | 50 % | 50 % |

### Typical annealed values

| Property | Value |
|---|---|
| Tensile strength | 620 MPa |
| Yield strength | 275 MPa |
| Elastic modulus | 193 GPa |
| Poisson's ratio | 0.27 to 0.30 |
| Elongation at break, 50 mm | 45 % |
| Hardness, Rockwell B | 85 |

Typical values are not acceptance criteria. Results shift with section size, forging reduction and test-piece location. Write the specification minimums into the purchase order, not the typical figures.

## Physical properties

| Property | Metric | Imperial |
|---|---|---|
| Density | 8.0 g/cm3 | 0.289 lb/in3 |
| Melting point | 1370 C | 2550 F |

## Forging and heat treatment

SUS 317 takes all the common hot-working methods. Stock is heated to 1149-1260 C and the pass schedule is planned so the workpiece leaves the press before it drops below 927 C, because working colder risks cracking and leaves residual strain that costs corrosion resistance later.

After forging or ring rolling, parts are solution annealed at 1010-1121 C and cooled. That returns carbides to solution and restores corrosion performance, so it is not optional on parts going into chloride service. The grade does not respond to hardening heat treatment; strength above the annealed condition comes only from cold work, followed by an anneal to relieve stress.

Machining is tougher going than 304. Chip breakers help, and a constant feed at moderate speed beats running slow. Discs and tube sheets are supplied proof-machined so ultrasonic probes sit on a clean surface.

Plant route: electric arc furnace with ladle refining and vacuum oxygen decarburisation, heats to 60 t; hydraulic presses at 6,300 t, 4,000 t and 2,000 t; five hammers from 750 kg to 5 t; radial-axial ring mills at 1 m, 3 m and 6 m; 14 heat-treatment furnaces including two 15 m well-type furnaces; vertical lathes to 5,000 mm swing and horizontal lathes to 14 m between centres.

## Product forms and size limits

| Form | Covers | Size limit |
|---|---|---|
| Seamless rolled rings | Rectangular and contoured section, gear ring blanks, slewing rings, bearing races | OD 50 to 6,000 mm |
| Forged rings | Upset and punched rings, retaining rings, valve seat rings | Outside the ring-mill envelope |
| Flanges | Weld neck, blind, slip-on, socket weld, lap joint, orifice, long weld neck | ASME B16.5, B16.47 |
| Bars and blocks | Round, flat and square bar, blanks for machined valve bodies | Press and lathe limits |
| Discs and tube sheets | Solid discs, tube sheets, covers, hubs | To 5,000 mm machined diameter |
| Shafts and spindles | Stepped shafts, eccentric shafts, spindles, rolls, pinions | To 14,000 mm turned length |
| Cylinders and sleeves | Bored hollows, sleeves, bushings, nozzles, heavy-wall pipe sections | To 1,600 x 10,000 mm bored |
| Valve parts | Bodies, bonnets, stems, seat rings, blocks, manifolds | To drawing |

Heaviest single piece is 30 t, set by the 60 t heat size and the 6,300 t press.

## Applications

317 is a pulp and paper, textile and chemical process grade before anything else. Common end uses for forged components:

- **Pulp and paper.** Digesters, liquor tanks, paper machine components, and the flanges, tube sheets and valve parts that go with them.
- **Chemical process.** Absorber towers, heat exchangers, pressure vessels, slurry tanks, stack liners, scrubber internals.
- **Refining and recovery.** Catalytic recovery systems, recuperators, forged pipe sections and tube sheets.
- **Valves and rotating parts.** Bodies, stems and seat rings for ball, gate, globe, check and plug valves; shafts, gear blanks and spindles.

## Designations and product standards

| System or product form | Designation |
|---|---|
| UNS | S31700 |
| AISI / SAE | 317, SAE 30317 |
| EN / DIN | 1.4449 |
| Forgings and piping components | ASTM A182 / ASME SA182 F317 |
| Plate and sheet | ASTM A240 / ASME SA240 |
| Bar and shapes | ASTM A276, A473, A479 |
| Pipe and tube | ASTM A312, A213, A249, A269 |
| Fittings | ASTM A403 / ASME SA403 |
| Low-carbon variant | 317L, UNS S31703 |

SUS 317 is the Japanese-style designation. Orders are normally placed against the UNS number or the ASTM product specification, and that is what the certificate references.

## Testing and certification

| Stage | Method | Reference |
|---|---|---|
| Chemical analysis | Optical emission spectrometry, infrared carbon and sulphur | ASTM E415, ASTM E1019 |
| Alloy verification | Handheld analyser, positive material identification | PMI |
| Tensile | 600 kN and 300 kN universal testing machines | ASTM A370, ISO 6892 |
| Impact | Pendulum machine with low-temperature bath | ASTM A370 |
| Ultrasonic | Digital flaw detection on proof-machined surfaces | ASTM A388, EN 10228-3 |
| Magnetic particle | Where applicable | ASTM E709 |
| Grain size | Metallography | ASTM E112 |
| Certificate | Mill test certificate, or witnessed by a third-party inspection body | EN 10204 3.1 / 3.2 |

Intergranular corrosion testing to ASTM A262 or G28 and pitting resistance to ASTM G48 are placed with an accredited outside laboratory and reported alongside the mill certificate. Request them at enquiry stage so they are scheduled before shipment.

## Frequently asked questions

**What is SUS 317 stainless steel?**
SUS 317 is the Japanese-style designation for the 317 molybdenum-bearing austenitic stainless steel, covered elsewhere as AISI 317, UNS S31700 and EN 1.4449. It runs 18.0-20.0 % chromium, 11.0-15.0 % nickel and 3.0-4.0 % molybdenum with carbon at 0.08 % maximum, making it a higher chromium, nickel and molybdenum version of 316 with more strength and better corrosion resistance.

**How does SUS 317 differ from 316?**
Molybdenum. SUS 317 carries 3.0-4.0 % against roughly 2-3 % in 316, with chromium and nickel also lifted. That buys resistance to pitting and crevice attack in chloride-bearing and moderately reducing service, which is why the grade shows up in pulp and paper and scrubber duty where 316 is borderline. It costs more, so confirm the service genuinely needs it.

**What does a SUS 317 forging have to test at?**
Under ASTM A182 Grade F317: 515 MPa tensile strength, 205 MPa yield strength, 30 % elongation in 50 mm or 4D, and 50 % reduction of area, all minimums. Published typical values for annealed material sit above that at roughly 620 MPa tensile, 275 MPa yield, 45 % elongation and Rockwell B 85.

**What are the forging and annealing temperatures?**
Hot work between 1149 and 1260 C, stopping before the piece falls below 927 C. Solution anneal at 1010-1121 C followed by cooling. The grade cannot be hardened by heat treatment, only by cold work.

**How large a SUS 317 part can be produced?**
Seamless rings roll to 6,000 mm outside diameter on the 6 m radial-axial mill, with 3 m and 1 m mills for smaller sizes. The heaviest single forging is 30 tonnes on 6,300 t, 4,000 t and 2,000 t presses. Two 15 m well furnaces allow long shafts to be quenched vertically; vertical lathes machine to 5,000 mm swing and horizontal lathes to 14 m between centres.

**Is there a minimum order, and how long does it take?**
Minimum order is 10 kg with no minimum piece count, so a single part is quotable. Lead time is 20 to 60 days from order confirmation, with SUS 317 at the lower end because it needs no remelting step.

**Can 317L be supplied instead?**
Yes. 317L (UNS S31703) is the low-carbon variant, normally chosen where components are welded and then exposed to aggressive service. State which of the two you need, because they are not interchangeable on a certificate.

## Request a quotation

Email sales@steelforgepieces.com with: grade or specification; dimensions or a drawing in PDF, DWG, DXF or STEP; quantity and expected repeat volume; delivery condition; heat treatment and testing requirements; certification and destination port. Price normally comes back within two working days.

---

Composition and property data compiled from published grade 317 (UNS S31700) datasheets and the ASTM A182 Grade F317 forging specification. Manufacturing capability, testing scope and commercial terms are this works' own. Figures are for guidance; confirm against the governing specification for your application. Reviewed 4 October 2026.