# PH15-7Mo Forgings (UNS S15700 / AISI Type 632)

PH15-7Mo is a chromium-nickel-molybdenum-aluminium semi-austenitic precipitation-hardening stainless steel, used where high strength and hardness are needed together with moderate corrosion resistance. It is 17-7PH with roughly 2 percent molybdenum substituted for 2 percent chromium, which raises strength at room and elevated temperature. Heat treated, it holds useful properties to about 482 C (900 F).

Also written PH 15-7 Mo, 15-7 Mo, 15-7Mo, 15-7 PH. Supplied by Jiangyin Jiangnan Metal Co., Ltd., an integrated melting works and open-die forging factory in Jiangyin, Jiangsu, China.

| Field | Detail |
|---|---|
| UNS | S15700 |
| AISI type | 632 |
| European cross-reference | EN 1.4532, X8CrNiMoAl15-7-2 |
| Class | Semi-austenitic precipitation-hardening stainless steel |
| Bars and forgings | AMS 5657 |
| Forgings | ASTM A705, ASTM A579 |
| Bars, forgings and forging stock | ASTM A461 |
| Bars, wire and shapes | ASTM A564 |
| Sheet, strip and plate | AMS 5520, ASTM A693, MIL-S-8955 |
| Weld wire | AMS 5812, AMS 5813 |
| Heat-treat conditions | A, TH 1050, RH 950; C and CH 900 are strip routes |
| Maximum useful service temperature | About 482 C (900 F) |
| Supplier | Jiangyin Jiangnan Metal Co., Ltd. |
| Plant | No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China |
| Telephone | +86 189 2135 9659 |
| Email | sales@steelforgepieces.com |
| Page | https://www.steelforgepieces.com/Stainless-Steel/PH15-7Mo.html |

## Designations and specifications

PH15-7Mo is published most often as a sheet and strip alloy, so the specification called up on a forging drawing matters. For bars and forgings the aerospace specification is AMS 5657. The list below is as given in the ATI 15-7 data sheet.

| Specification | Product form |
|---|---|
| AMS 5520 | Sheet, strip and plate |
| AMS 5657 | Bars and forgings |
| AMS 5812, AMS 5813 | Weld wire |
| ASTM A461 | Bars, forgings and forging stock |
| ASTM A564 | Bars, wire and shapes |
| ASTM A579 | Forgings |
| ASTM A693 | Plate, sheet and strip |
| ASTM A705 | Forgings |
| MIL-S-8955 | Plate, sheet and strip |

ASTM B564 is sometimes quoted against this grade in error. That specification covers nickel and nickel-copper alloy forgings for general corrosion service and pressure vessel use, and contains no stainless steel grades.

## Chemical composition

Composition in weight percent per AMS 5520. Single figures are maxima.

| Element | Weight percent | Function |
|---|---|---|
| Carbon | 0.09 max | Held low to protect corrosion resistance and toughness |
| Chromium | 14.00 to 16.00 | Passivity; about 2 percent lower than 17-7PH to make room for molybdenum |
| Nickel | 6.50 to 7.75 | Stabilises the austenite of Condition A |
| Molybdenum | 2.00 to 3.00 | Raises strength at room and elevated temperature |
| Aluminium | 0.75 to 1.50 | The hardening element, and a reactive one, which is why welding uses inert gas |
| Manganese | 1.00 max | Deoxidiser |
| Silicon | 1.00 max | Deoxidiser |
| Phosphorus | 0.040 max | Residual |
| Sulfur | 0.030 max | Residual |
| Iron | Balance | Matrix |

Forging stock is melted in the electric arc furnace, refined in the ladle furnace and vacuum decarburised. Electroslag remelted material is available where a remelted grade is specified. ATI notes that vacuum arc or electroslag remelted S15700 is supplied for a further increase in fatigue resistance in applications subject to cyclic stresses.

## Heat treatment

PH15-7Mo cannot be hardened in one step from the annealed condition. Two things have to follow Condition A: a treatment that lets the relatively stable austenite transform to martensite, then a precipitation-hardening treatment. This is the main practical difference from 17-4PH and the usual source of ordering mistakes.

| Condition | Route | Outcome |
|---|---|---|
| A | Solution treat at 1950 F (1066 C), air cool | Structure primarily austenite, relatively low strength, weakly ferromagnetic. Formability and machining are easiest here |
| TH 1050 | From Condition A: hold at 1400 F (760 C) for 90 minutes, cool to 55 F (13 C) within one hour and hold 30 minutes, then age at 1050 F (565 C) for 90 minutes and air cool | Martensite transformation occurs near room temperature, so no cryogenic plant is needed. The normal route for forged and machined parts |
| RH 950 | From Condition A: hold at 1750 F (955 C) for 10 minutes, cool to room temperature, then within one hour cool to minus 100 F (minus 73 C), hold 8 hours, warm in air, then age at 950 F (510 C) for 90 minutes and air cool | Highest strength without cold work. The transformation is not complete until the sub-zero hold is finished |
| C and CH 900 | Condition A is transformed to martensite at the mill by cold reduction to Condition C, the part is fabricated, then aged at 900 F (482 C) for 60 minutes | The highest strength condition, achieved at the cost of low tensile ductility. A strip route, not applicable to forgings |

Because both hardening steps run at low temperature, movement is far smaller than in a conventional quench and temper cycle, which is why parts are finish-machined in Condition A and hardened afterwards. ATI warns that the precipitation reaction can be driven past peak strength by high temperature or excessive time at the ageing temperature, so a hotter or longer cycle than the standard one produces lower strength, not higher.

## Mechanical properties

Both tables below are sheet and strip data, because that is the form in which this grade is most fully published. Acceptance limits for bar and forging come from AMS 5657 or ASTM A564 for the ordered section, and fall as section thickness rises, so they are agreed at enquiry rather than read across from strip figures.

AMS 5520 minimum properties, sheet and strip.

| Condition | Thickness, in | Tensile, ksi | Yield, ksi | Elongation, % | Hardness |
|---|---|---|---|---|---|
| Solution treated | below 0.005 | 150 max | 65 max | 25 | 100 HB max |
| TH 1050 | 0.010 to 0.020 | 190 | 170 | 4 | 40 HRC |
| TH 1050 | 0.020 to 0.1875 | 190 | 170 | 5 | 40 HRC |
| TH 1050 | 0.1875 to 0.500 | 190 | 170 | 6 | 40 HRC |
| RH 950 | 0.010 to 0.020 | 225 | 220 | 3 | 45 HRC |
| RH 950 | 0.020 to 0.1875 | 225 | 220 | 4 | 45 HRC |
| RH 950 | 0.1875 to 0.500 | 225 | 220 | 5 | 45 HRC |
| Condition C | - | 200 | 175 | 1 | 41 HRC |
| CH 900 | - | 240 | 230 | 1 | 46 HRC |

Typical room-temperature properties, sheet and strip, per ATI.

| Property | Condition A | TH 1050 | RH 950 |
|---|---|---|---|
| 0.2 % yield strength, psi (MPa) | 55,000 (380) | 200,000 (1380) | 220,000 (1515) |
| Ultimate tensile strength, psi (MPa) | 125,000 (860) | 210,000 (1450) | 245,000 (1690) |
| Elongation, % | 30 | 6 | 6 |
| Hardness, Rockwell | 88 HRB | 43 HRC | 48 HRC |
| Modulus of elasticity, 10^6 psi (GPa) | 28 (195) | 28 (195) | 28 (195) |

Once hardened this is a low-ductility material, and that governs whether it suits a given forged part. ASTM A564 scopes these grades for service to 600 F (315 C), extended to 700 F (370 C) for Type 632.

Condition RH 950, S15700 against S17700, short-time elevated-temperature tensile data per ATI.

| Temperature | Property | S15700 | S17700 |
|---|---|---|---|
| 70 F (21 C) | 0.2 % yield, psi (MPa) | 220,000 (1515) | 200,000 (1380) |
| 70 F (21 C) | Tensile, psi (MPa) | 245,000 (1690) | 225,000 (1550) |
| 300 F (149 C) | 0.2 % yield, psi (MPa) | 205,000 (1415) | 192,000 (1325) |
| 300 F (149 C) | Tensile, psi (MPa) | 228,000 (1570) | 208,000 (1435) |
| 600 F (316 C) | 0.2 % yield, psi (MPa) | 178,000 (1225) | 169,000 (1165) |
| 600 F (316 C) | Tensile, psi (MPa) | 205,000 (1415) | 189,000 (1305) |

## Physical properties

Per ATI.

| Property | Condition A | TH 1050 | RH 950 |
|---|---|---|---|
| Density, lb/in3 (g/cm3) | 0.282 (7.80) | 0.277 (7.67) | 0.277 (7.67) |
| Expansion 70 to 200 F, 10^-6/F (10^-6/C) | 8.0 (14.4) | 6.1 (11.0) | 5.0 (9.0) |
| Expansion 70 to 400 F, 10^-6/F (10^-6/C) | 8.0 (14.4) | 6.1 (11.0) | 5.4 (9.7) |
| Expansion 70 to 600 F, 10^-6/F (10^-6/C) | 8.5 (15.3) | 6.1 (11.0) | 5.6 (10.1) |
| Magnetic response | Weakly ferromagnetic | Strongly ferromagnetic | Strongly ferromagnetic |

Thermal conductivity is 8.7 Btu-ft/h-ft2-F (15.1 W/m-K) at 70 F, rising to 9.3 (16.2) at 200 F. Electrical resistivity is approximately 82 microhm-cm in the annealed or hardened conditions.

## Section size limits

ASTM A564 states in its scope that Types 631 and 632 contain a large amount of ferrite in the microstructure and can have low ductility in forgings and larger diameter bars, and that applications should be limited to small diameter bar.

If a drawing calls for a large seamless rolled ring, a heavy tube sheet, a thick pressure-retaining flange, a crankshaft or a mill component in PH15-7Mo, a different precipitation-hardening grade is usually the right answer.

| Grade | UNS and type | Where it fits |
|---|---|---|
| PH15-7Mo | S15700, 632 | Highest strength of the semi-austenitic pair, useful to 482 C. Keep to small diameter bar and compact forged parts |
| 17-7PH | S17700, 631 | The same family without molybdenum. The same ferrite and section caution applies |
| 17-4PH | S17400, 630 | The workhorse martensitic grade for heavy forgings, hardened in a single ageing step |
| 15-5PH | S15500, XM-12 | 17-4PH rebalanced for better transverse toughness in heavy sections |
| PH13-8Mo | S13800, XM-13 | Premium-melt grade where high transverse toughness and high strength are both required |

## Corrosion, welding, machining

ATI reports that corrosion resistance approaches that of Type 304 in most media and is generally superior to the hardenable 400 series stainless steels. High Temp Metals puts the same grade a little lower, rating general corrosion resistance in TH 1050 and RH 950 as superior to the standard hardenable types such as 410, 420 and 431 but not as good as Type 304. The second is the safer design assumption.

On welding, ATI describes the alloy as weldable by conventional inert-gas methods with behaviour similar to 17-7PH, and counts the absence of the preheating and post-weld annealing needed for conventional hardenable stainless steels among its useful features. Inert-gas methods protect against loss of aluminium, and molybdenum raises the amount of ferrite in the weld deposit compared with 17-7PH. High Temp Metals is more cautious, stating that the alloy is generally considered to have poorer weldability than 17-4PH, that the high aluminium content degrades penetration and increases weld slag formation during arc welding, and that both austenite conditioning and precipitation hardening are required after welding to reach high strength levels. Filler is normally WP 15-7 Mo or W 17-7 PH.

Machine in Condition A. In that state the material forms much like Type 301, work-hardens quickly, may need intermediate annealing for deep drawing or intricate shapes, and springs back similarly to Type 301. Once aged to RH 950 the material is around 48 HRC and is a grinding or EDM job rather than a turning and drilling one.

## Product forms

- Forged round bars, and billets or bars for reforging.
- Forged discs, blanks and compact rings in small diameters and moderate sections.
- Forged sleeves, bushings and spacers, rough turned or finish machined.
- Valve components: stems, seat rings, plugs and small bodies for ball, gate, globe, check and plug valves.
- Shafts, spindles and pins for pumps, compressors and instrumentation.
- Near-net machined parts in Condition A for customer ageing, or aged to TH 1050 or RH 950 before despatch.

## Testing and certification

Chemical analysis and mechanical testing follow the methods called up by the ordered specification, with yield taken at 0.2 percent offset. Where volumetric examination is specified the works tests to EN 10228-3, SEP 1921 or ASTM A388. Certification is issued to EN 10204 type 3.1, or type 3.2 with third-party witness. Hardness surveys, dimensional reports, positive material identification, liquid penetrant examination and transverse-direction testing are available on request. Transverse properties should be specified explicitly, since standard practice only calls for them above a certain bar diameter.

Minimum order 10 kg, single pieces accepted. Normal lead time 20 to 60 days depending on section, heat treatment and examination scope.

## Questions

**Is PH15-7Mo martensitic or semi-austenitic?** Semi-austenitic. It is furnished annealed in Condition A, where the structure is primarily austenite and strength is relatively low. The austenite is transformed to martensite afterwards, either by conditioning and cooling or by cold reduction at the mill to Condition C, before the final ageing step. It is not a martensitic grade in the way 17-4PH is.

**Which standard should go on the drawing?** AMS 5657 for bars and forgings, ASTM A705 or ASTM A579 for forgings, ASTM A461 for bars, forgings and forging stock, or ASTM A564 for bars, wire and shapes. ASTM B564 covers nickel and nickel-copper alloy forgings and does not apply.

**Why specify PH15-7Mo rather than 17-7PH?** Molybdenum. The grade is 17-7PH with about 2 percent molybdenum in place of 2 percent chromium, which gives somewhat higher strength at room and elevated temperature. At 600 F in RH 950, ATI gives S15700 a yield of 178,000 psi against 169,000 psi for S17700.

**Can large PH15-7Mo rolled rings or tube sheets be made?** They can be forged, but ASTM A564 limits Type 632 applications to small diameter bar because of ferrite content and low ductility in forgings and larger sections. For large rings, heavy discs and thick pressure parts, 17-4PH, 15-5PH or PH13-8Mo give comparable strength with better section ductility and toughness.

**Which condition should be ordered?** Condition A in almost every case: solution treated at 1950 F and air cooled, machined, then aged. TH 1050 needs no cryogenic equipment. RH 950 requires cooling to minus 100 F and an 8 hour hold.

## Sources

1. ATI 15-7 Semi-Austenitic Stainless Steel (UNS S15700) technical data sheet, version 1, 2014.
2. Aircraft Materials, PH 15-7 Mo stainless steel data sheet. AMS 5520 heat-treatment cycles and minimum properties by thickness.
3. ASTM A564/A564M, Standard Specification for Hot-Rolled and Cold-Finished Age-Hardening Stainless Steel Bars and Shapes.
4. ASTM A705/A705M, Standard Specification for Age-Hardening Stainless Steel Forgings.
5. ASTM B564, Standard Specification for Nickel Alloy Forgings. Cited only to show this grade falls outside its scope.
6. High Temp Metals, 15-7 Mo technical data.
7. AZoM, Stainless Steel Grade 15-7Mo (UNS S15700).
8. ASM International, Alloy Digest, Armco PH 15-7 Mo stainless steel.

Figures are reproduced from the specifications and data sheets listed above for information. They are not a warranty of properties for a particular part or section size, and published data is typical rather than a design minimum unless the specification states otherwise. Acceptance values are agreed against the governing specification at order.