**AISI 632 is a chromium-nickel-molybdenum-aluminium semi-austenitic precipitation hardening stainless steel, designated UNS S15700 and sold as PH15-7Mo.** It is 17-7 PH with about 2 percent molybdenum substituted for about 2 percent chromium, which raises strength at room temperature and at elevated temperature.

Jiangyin Jiangnan Metal Co., Ltd. forges the grade into rings, seamless rolled rings, flanges, bars, discs, sleeves and shafts to ASTM A564, ASTM A579 and ASTM A705 Grade 632 and AMS 5657. The steel is melted on site, so the certificate traces back to a melt number rather than to a purchased billet.

Source page: https://www.steelforgepieces.com/Stainless-Steel/AISI-632.html

## Grade summary

| Field | Detail |
|---|---|
| Designations | AISI 632, UNS S15700, PH15-7Mo, 15-7 Mo, 15-7 PH, EN 1.4532, X8CrNiMoAl15-7-2 |
| Class | Semi-austenitic precipitation hardening stainless steel |
| Nominal composition | 15 Cr, 7 Ni, 2 to 3 Mo, 1 Al, balance Fe |
| Forging specifications | ASTM A564, A579, A705 Grade 632, ASTM A461, AMS 5657 |
| Supply conditions | Condition A annealed, TH 1050, RH 950 on enquiry |
| Typical strength | to about 1448 MPa tensile in TH 1050, about 1690 MPa in RH 950 |
| Maximum service temperature | about 482 C |
| Melting | EF, LF, VOD. VAR or ESR remelt available |
| Certification | EN 10204 3.1, or 3.2 witnessed |
| Minimum order | 10 kg, no minimum piece count |
| Lead time | 20 to 60 days |

## What the grade is for

AISI 632 earns its place where a 400-series martensitic grade would be strong enough but corrodes too readily, and an austenitic grade resists corrosion well enough but cannot carry the load.

The semi-austenitic precipitation hardening grades are specified as much for how they are processed as for what they end up at. The alloy is delivered soft and austenitic, in Condition A, where it forges and machines without difficulty. Strength comes later, from low-temperature ageing. Because there is no high-temperature quench in the hardening sequence, distortion stays low. On a 2 metre rolled ring or a 6 metre shaft, that is the difference between a part that can be finish-machined to drawing and one that has to be straightened first.

The grade has a long record in aerospace work and in spring-type components needing high strength. Material taken through vacuum arc or electroslag remelting gives further improvement in fatigue resistance, which is the usual choice for rotating and spring applications. Both remelting routes run in this works, on a 6 t vacuum arc furnace and 3 t and 6 t protective-atmosphere electroslag furnaces.

## Chemical composition

Weight percent. Single figures are maxima.

| Element | Min | Max | Function |
|---|---|---|---|
| Chromium, Cr | 14.00 | 16.00 | Passive film, corrosion resistance |
| Nickel, Ni | 6.50 | 7.75 | Austenite stability in Condition A |
| Molybdenum, Mo | 2.00 | 3.00 | Strength, pitting resistance |
| Aluminium, Al | 0.75 | 1.50 | Hardening element |
| Carbon, C | - | 0.09 | Residual |
| Manganese, Mn | - | 1.00 | Residual |
| Silicon, Si | - | 1.00 | Residual |
| Phosphorus, P | - | 0.040 | Impurity |
| Sulphur, S | - | 0.040 | Impurity |
| Iron, Fe | Balance | Balance | Matrix |

Published limits for sulphur vary between sources, with 0.040 and 0.030 percent maximum both in circulation. State the governing specification on the order and the heat will be aimed at that limit. Because melting is on site, chemistry is set at the furnace rather than accepted as delivered.

Aluminium is the element that makes the grade work, and it is reactive. That single fact drives both the melting practice and the welding practice.

## Mechanical properties by condition

Typical published room-temperature values, for information only, not specification minima.

| Condition | 0.2% yield | Tensile | Elongation | Hardness | Available on forgings |
|---|---|---|---|---|---|
| A, annealed | 380 MPa / 55 ksi | 896 MPa / 130 ksi | 30 to 35% | 88 HRB | Yes, supply and machining condition |
| TH 1050 | 1380 MPa / 200 ksi | 1448 MPa / 210 ksi | 7% | 43 to 44 HRC | Yes, standard hardened condition |
| RH 950 | 1515 MPa / 220 ksi | 1690 MPa / 245 ksi | 6% | 48 HRC | On enquiry |
| C, cold reduced | 1310 MPa / 190 ksi | 1517 MPa / 220 ksi | 5% | 45 HRC | No, strip condition |
| CH 900 | 1793 MPa / 260 ksi | 1828 MPa / 265 ksi | 2% | 50 HRC | No, requires cold reduction |

**On CH 900 and forgings.** CH 900 is the highest-strength condition this alloy reaches, but it is obtained by heavy cold reduction to Condition C followed by ageing near 482 C. Cold reduction of that order is a strip-mill operation and cannot be applied to a forged ring, shaft or flange. Any quotation offering forgings in CH 900 is worth questioning. For forged product the practical ceiling is RH 950.

### Elevated temperature, against 17-7 PH

Short-time tensile data, Condition RH 950, typical published values.

| Temperature | S15700 yield | S17700 yield | S15700 tensile | S17700 tensile |
|---|---|---|---|---|
| 21 C | 1515 MPa | 1380 MPa | 1690 MPa | 1550 MPa |
| 149 C | 1415 MPa | 1325 MPa | 1570 MPa | 1435 MPa |
| 316 C | 1225 MPa | 1165 MPa | 1415 MPa | 1305 MPa |

Useful properties run to roughly 482 C. Past that the hardening precipitates coarsen and strength drops away, which puts the grade out of contention for sustained hotter service. For that duty the enquiry should move to nickel alloys such as Inconel 617 or Incoloy 800H.

## Physical properties

| Property | Condition A | TH 1050 | RH 950 |
|---|---|---|---|
| Density | 7.80 g/cm3 | 7.68 g/cm3 | 7.67 g/cm3 |
| Modulus of elasticity | - | 196 GPa | 200 GPa |
| Thermal conductivity at 21 C | - | 15.1 W/m.K | 15.1 W/m.K |
| Thermal conductivity at 316 C | - | 19.7 W/m.K | 19.2 W/m.K |
| Mean expansion, 21 to 93 C | 14.4 um/m.K | 11.0 um/m.K | 9.0 um/m.K |
| Mean expansion, 21 to 316 C | 15.3 um/m.K | 11.0 um/m.K | 10.1 um/m.K |
| Electrical resistivity | about 82 uOhm.cm | about 82 uOhm.cm | about 82 uOhm.cm |
| Magnetic response | Weakly magnetic | Magnetic | Magnetic |

The density shift between Condition A and the aged conditions, and the drop in expansion coefficient, both follow from the austenite-to-martensite transformation. Allow for the dimensional change when a part is machined in Condition A and aged afterwards.

## Heat treatment

Hardening needs three steps in order: condition the austenite, transform it to martensite, then precipitation harden. The two routes differ only in how the transformation is forced.

**Condition TH 1050.** Austenite conditioning near 760 C, typically held around 90 minutes, destabilises the austenite so martensite forms at about room temperature on cooling. Precipitation hardening follows near 565 C for about 90 minutes, air cooled. No sub-zero equipment is involved, which makes TH 1050 the economical and dependable route for heavy forged sections. This is the hardened condition supplied as standard.

**Condition RH 950.** Austenite conditioning near 955 C, then a hold near minus 73 C for about 8 hours to carry the transformation to completion, then precipitation hardening near 510 C. RH 950 gives the higher strength of the two forging conditions. The route needs a sub-zero hold, so raise it at enquiry stage and have the chamber capacity confirmed against your section size and quantity before the order is placed. TH 1050 carries no such constraint.

**Over-ageing.** The precipitation reaction can be pushed past peak strength by too high a temperature or too long at temperature, and the result is lower strength, not higher. Furnace uniformity surveys and soak-time control on heavy sections decide whether a ring conforms or goes to scrap. Ageing runs in car-bottom furnaces with chamber sizes to 8,000 by 2,000 by 2,000 mm, with charted records issued against each heat-treatment lot.

## Corrosion resistance, machining, welding

**Corrosion resistance.** In the hardened conditions AISI 632 resists corrosion better than the hardenable 400-series martensitic grades, Type 410, 420 and 431 among them. Against Type 304 the published positions differ in emphasis: some mill data describes the grade as approaching Type 304 in most media, other data describes it as not equal to Type 304. Both readings point the same way, so treat 632 as close to but not better than 304. Specify it for very high strength with moderate corrosion resistance, not as a replacement for 304, and not for aggressive chloride service where duplex or super-duplex grades belong.

**Machining.** Machine in Condition A wherever the tolerance scheme allows. In that condition the alloy work hardens quickly, so rigid setups, positive rake, sharp tooling and steady feed all matter. Once aged, hardness sits at 43 to 48 HRC and turning, drilling and milling become slow and tool-intensive. The normal production order is forge, anneal, rough machine with an ageing allowance, heat treat, then finish machine or grind only the features that need it.

**Welding.** The grade welds by conventional inert-gas methods and behaves much like 17-7 PH. Gas shielding is not optional, because the hardening response depends on aluminium and aluminium is lost readily to oxidation. The high aluminium content reduces arc penetration and promotes weld slag, and the molybdenum addition raises ferrite in the deposit compared with 17-7 PH. Some sources rate the grade as harder to weld than 17-4 PH for these reasons. Where filler is needed, WP 15-7 Mo or W 17-7 PH is usually called for, and both austenite conditioning and precipitation hardening have to follow welding if the joint is to reach full strength. The grade does not need the preheat and post-weld anneal used on conventional hardenable stainless steels.

## Specifications

| Specification | Product form | Applies to forgings |
|---|---|---|
| ASTM A564 Grade 632 | Bars, forgings, forging stock | Yes, primary |
| ASTM A579 Grade 632 | Forgings | Yes, primary |
| ASTM A705 Grade 632 | Forgings | Yes, primary |
| ASTM A461 | Forged bolting | Yes |
| AMS 5657 | Bars and forgings | Yes |
| AMS 5520 | Sheet, strip, plate | No |
| ASTM A693 Grade 632 | Plate, sheet, strip | No |
| MIL-S-8955 | Plate, sheet, strip | No |
| AMS 5812, AMS 5813 | Weld wire | Filler metal only |
| EN 1.4532, X8CrNiMoAl15-7-2 | European designation | Cross-reference |

**A correction worth making.** AISI 632 forgings are sometimes quoted and certified against ASTM B564. That is wrong. ASTM B564 covers nickel-alloy forgings and does not include UNS S15700. If a quotation or a mill certificate cites B564 against AISI 632, ask for it to be reissued against A564, A579, A705 or AMS 5657. The same error appears on a number of supplier pages for this grade.

Watch the designation as well as the standard. AISI 632 is not 15-5 PH (S15500) and not 17-7 PH (S17700), though the names sit close together. Quote the UNS number on the order and the ambiguity disappears.

## Product forms

Produced to customer drawing or written specification in AISI 632 / UNS S15700: seamless rolled rings, forged rings, retaining rings, flanges, round bars, discs and tube sheets, sleeves and bushings, shafts and spindles, eccentric shafts, hollow bars and cylinders, valve stems and seat rings, valve bodies and blocks, gear blanks, nozzles, blocks and blanks.

| Item | Limit | Set by |
|---|---|---|
| Seamless rolled rings | OD 50 to 6,000 mm | 6 m, 3 m and 1 m radial-axial ring mills |
| Forged shafts | to 14,000 mm turned length | C61160 horizontal lathe, 15 m well furnace |
| Discs, tube sheets, blocks | to 5,000 mm machined diameter | 5,000 mm vertical lathe |
| Bored cylinders and hollow shafts | to 1,600 mm dia by 10,000 mm | CNC deep-hole drilling machine |
| Single-piece weight | to 30,000 kg | 60 t heat size, 6,300 t press |
| Minimum order | 10 kg | No minimum piece count |
| Lead time | 20 to 60 days | Longer where a remelting step is specified |

### Where the grade is used

The strength and distortion behaviour put AISI 632 into aerospace components and spring-type parts, which is where the alloy built its record. In process and energy equipment the same properties suit pump and plunger-pump shafts, valve stems and seat rings for ball, gate, globe, check and plug valves, flanges and tube sheets for heat exchangers and pressure vessels, and sleeves, discs and bushings for compressors and generators. For rotating or cyclically loaded parts, specify vacuum arc or electroslag remelted material on the enquiry, since the remelting step affects both price and delivery.

## Testing and certification

The steel is melted here, so chemistry is verified at the furnace instead of being carried over from a billet supplier's certificate.

| Discipline | Equipment | Standard |
|---|---|---|
| Chemical analysis | SPECTROTEST TXC25 optical emission spectrometer | ASTM E415 |
| Carbon and sulphur | HIR-9440D infrared analyser | ASTM E1019 |
| Alloy verification | X-Mwt3000TX handheld analyser | Positive material identification |
| Tensile | WE-600B 600 kN, WDW-300 | ASTM A370, ISO 6892 |
| Impact | JBN-300 with DWC-60 low-temperature bath | ASTM A370, to minus 60 C |
| Hardness | TH140 Leeb tester | ASTM A956, converted per ASTM E140 |
| Ultrasonic | PXUT-3300, USM35XS, CTS-22 | ASTM A388, EN 10228-3 |
| Magnetic particle | CYE-3A | ASTM E709 |
| Grain size | XJP-6A microscope with preparation line | ASTM E112 |

Hardness acceptance on aged material deserves a word at order stage. Portable Leeb readings converted per ASTM E140 are adequate for process control, but where a specification calls for bench Rockwell or Brinell measurement, that is placed with an accredited third-party laboratory and the report issued alongside the mill certificate. Corrosion testing to ASTM A262, G28 or G48 is handled the same way.

The works holds CCS, BV, DNV, LR and NK approvals. Certification is issued to EN 10204 3.1, or to EN 10204 3.2 witnessed by BV, DNV, LR, SGS, TUV or the customer's own inspector. Chemical analysis, tensile and hardness results, heat-treatment charts and ultrasonic reports are supplied per heat and per heat-treatment lot, traceable from the melt number through to shipment.

## Frequently asked questions

### What is AISI 632 stainless steel?

A chromium-nickel-molybdenum-aluminium semi-austenitic precipitation hardening stainless steel, designated UNS S15700 and sold as PH15-7Mo or 15-7 Mo. Composition runs 14.00 to 16.00 percent chromium, 6.50 to 7.75 percent nickel, 2.00 to 3.00 percent molybdenum and 0.75 to 1.50 percent aluminium, balance iron. It is derived from 17-7 PH by substituting about 2 percent molybdenum for about 2 percent chromium, which raises strength at room temperature and at temperature.

### Is AISI 632 the same as PH15-7Mo, 15-7 PH and 1.4532?

Yes, those are designations for one alloy. AISI 632 is the AISI type number, UNS S15700 the unified number, PH15-7Mo and 15-7 Mo the common trade names, and 1.4532 or X8CrNiMoAl15-7-2 the European designation. It is not 15-5 PH (S15500) and not 17-7 PH (S17700), which are different alloys with similar-looking names.

### Which standard should AISI 632 forgings be ordered against?

ASTM A564 Grade 632 for bars, forgings and forging stock, ASTM A579 Grade 632 or ASTM A705 Grade 632 for forgings, ASTM A461 for forged bolting, or AMS 5657 for bars and forgings. AMS 5520 and ASTM A693 cover sheet, strip and plate and are not forging specifications. ASTM B564 is a nickel-alloy forging specification and does not cover this grade, so a certificate citing it should be reissued.

### What heat treatment conditions are available for AISI 632 forgings?

Condition A is the annealed, soft austenitic condition used for forging and rough machining. Condition TH 1050 uses austenite conditioning near 760 C followed by precipitation hardening near 565 C and needs no sub-zero equipment, which makes it the standard hardened condition for forgings. Condition RH 950 uses austenite conditioning near 955 C, a hold near minus 73 C, then precipitation hardening near 510 C, and gives higher strength. Condition CH 900 requires heavy cold reduction and is a strip condition that cannot be reached on an open-die forging.

### How strong is AISI 632 compared with 17-7 PH?

Stronger in the same condition. In Condition RH 950 at room temperature, typical published values for S15700 are about 1515 MPa yield and 1690 MPa tensile, against about 1380 MPa yield and 1550 MPa tensile for S17700. The margin holds at temperature: at 316 C in RH 950, S15700 gives about 1225 MPa yield against about 1165 MPa for S17700.

### Is the corrosion resistance better than 410 or 420 stainless steel?

Yes. In the hardened conditions AISI 632 resists corrosion better than the hardenable 400-series martensitic grades such as Type 410, 420 and 431. Against Type 304 the published positions differ, with some mill data describing 632 as approaching Type 304 in most media and other data describing it as not equal to Type 304. Treat the grade as close to but not better than 304, and do not substitute it for 304 or for duplex grades in aggressive chloride service.

### How does the grade compare with 17-4 PH for forged parts?

17-4 PH is martensitic and hardens in one ageing step, so it is simpler to process and is better regarded for welding. AISI 632 is semi-austenitic, needs austenite conditioning before ageing, and reaches considerably higher strength with less distortion through heat treatment. Choose 632 when strength or distortion control decides the part, and 17-4 PH when fabrication and welding decide it.

### Can AISI 632 be welded?

Yes, by inert-gas methods, and it behaves broadly like 17-7 PH. Gas shielding is essential because the hardening response depends on aluminium and aluminium oxidises readily. The high aluminium content reduces arc penetration and promotes weld slag, and the molybdenum raises ferrite in the deposit compared with 17-7 PH. WP 15-7 Mo or W 17-7 PH filler is normally specified, and both austenite conditioning and precipitation hardening must follow welding if full strength is needed in the joint. Preheat and post-weld annealing of the kind used on conventional hardenable stainless steels are not required.

### What is the maximum service temperature?

Roughly 482 C for useful mechanical properties. In Condition RH 950 at 316 C the grade still shows about 1225 MPa yield strength. Above about 482 C the hardening precipitates coarsen and strength falls, so the selection should move to a different alloy family.

### What size and weight can you forge in this grade?

Rings roll to 6,000 mm outside diameter and down to 50 mm by the upset-and-punch route. The heaviest single forging is 30 tonnes, worked on 6,300 t, 4,000 t and 2,000 t presses. Shafts turn to 14,000 mm, discs to 5,000 mm diameter. Minimum order is 10 kg with no minimum piece count. Grade-specific limits depend on section size and the heat treatment specified, so send the drawing and they will be confirmed against the quotation.

### How long does an AISI 632 forging take?

20 to 60 days from order confirmation. Standard melting through the electric arc furnace with ladle refining and vacuum decarburisation sits at the lower end. Specifying vacuum arc or electroslag remelted material, witnessed inspection to EN 10204 3.2, or testing placed with an outside laboratory moves the date out, so flag all three at enquiry stage.

### Who supplies AISI 632 open-die forgings?

Jiangyin Jiangnan Metal Co., Ltd., an integrated melting works and open-die forging factory at No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China, operating since 1997 with 460 staff. The works melts its own steel, holds CCS, BV, DNV, LR and NK approvals, accepts orders from 10 kg with no minimum piece count and quotes 20 to 60 days. Contact +86 189 2135 9659 or sales@steelforgepieces.com.

## Related grades

17-7 PH (UNS S17700): https://www.steelforgepieces.com/Stainless-Steel/17-7ph.html
15-5 PH (UNS S15500): https://www.steelforgepieces.com/Stainless-Steel/15-5ph.html
PH 13-8 Mo (UNS S13800): https://www.steelforgepieces.com/Stainless-Steel/PH13-8Mo.html
AISI 422: https://www.steelforgepieces.com/Stainless-Steel/AISI-422.html
All stainless steel grades: https://www.steelforgepieces.com/Stainless-Steel/

## Request a quotation

Send the grade or specification, the dimensions or a drawing in PDF, DWG, DXF or STEP, the quantity, the delivery condition, the heat treatment and testing requirements and the destination port. A complete enquiry is normally priced within two working days.

**Jiangyin Jiangnan Metal Co., Ltd.**
No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China, 214423
Telephone, WhatsApp and WeChat: +86 189 2135 9659
Email: sales@steelforgepieces.com
Hours: Monday to Saturday, 08:00 to 17:30 China Standard Time, UTC+8

---

Technical data is compiled from published mill data sheets for UNS S15700 and is given for information only. It is not a specification and not a warranty for any particular design or application. Order acceptance is against the minima of the applicable ASTM or AMS specification for the relevant product form and section size.

Copyright 1997 to 2026 Jiangyin Jiangnan Metal Co., Ltd. Page reviewed 2 October 2026.