# AISI 444 Forgings: UNS S44400 / SUS 444 / EN 1.4521 (X2CrMoTi18-2)

Supplier: Jiangyin Jiangnan Metal Co., Ltd., open-die forging factory
Address: No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
Tel: +86-189-2135-9659
Email: sales@steelforgepieces.com
Source page: https://www.steelforgepieces.com/Stainless-Steel/AISI-444.html

AISI 444 is a stabilised ferritic stainless steel with about 18% chromium and 2% molybdenum, and very low carbon and nitrogen. The Cleveland-Cliffs product datasheet for Type 444 states that it gives pitting and crevice corrosion resistance better than most ferritic stainless steels and some austenitic stainless steels, matches Type 304 in many corrosion environments, and beats both Type 304 and Type 316 on chloride stress corrosion cracking. Jiangyin Jiangnan Metal forges this grade into rings, sleeves, shafts and discs for hot-water tanks, heat exchangers, and food, brewing and wine-making plant.

## Key facts

| Item | Value |
|---|---|
| UNS number | S44400 (S44401 also listed for the ASTM variant) |
| EN number and name | 1.4521 / X2CrMoTi18-2 |
| JIS (Japan) | SUS444, SUS444TP |
| GB (China) | 019Cr19Mo2NbTi, 00Cr18Mo2 |
| Other designations | SS 2326, UNE F3123, AS 1449 grade 444, SAE J405 S44400 |
| Structure | Ferritic, magnetic, not hardenable by heat treatment |
| Product standards | ASTM A240 (plate, sheet, strip), ASTM A268 (tubing), EN 10028-7 (flat products for pressure purposes) |
| PREN | About 25 (Virgamet); 23.3 to 28.3 (ModulusMetal) |

## Chemical composition, weight percent

ASTM A240 S44400 is dual-stabilised with titanium and niobium and controls the combined Ti plus Nb content. EN 1.4521 specifies titanium only. The two are not interchangeable on a purchase order.

| Element | ASTM A240, UNS S44400 | EN 1.4521, X2CrMoTi18-2 | JIS SUS444 |
|---|---|---|---|
| C | 0.025 max | 0.025 max | 0.025 max |
| Si | 1.00 max | 1.00 max | 1.00 max |
| Mn | 1.00 max | 1.00 max | 1.00 max |
| P | 0.04 max | 0.04 max | 0.04 max |
| S | 0.03 max | 0.015 max | 0.03 max |
| Cr | 17.5 to 19.5 | 17.0 to 20.0 | 17.0 to 20.0 |
| Mo | 1.75 to 2.5 | 1.80 to 2.50 | 1.75 to 2.50 |
| Ni | 1.00 max | not specified | not specified |
| N | 0.035 max | 0.030 max | 0.025 max |
| Ti / Nb | Ti + Nb: 0.20 + 4(C+N) min, 0.80 max | Ti: 0.15 to 0.80, i.e. 4(C+N) + 0.15 | not specified |
| Fe | Balance | Balance | Balance |

Sources: Cleveland-Cliffs Type 444 datasheet for the ASTM column; Virgamet and Metalcor for the EN and JIS columns.

Ordering note: stabilisation chemistry is the most common reason 444 material gets rejected on receipt. If the specification is ASTM A240 or A268, the heat has to satisfy the Ti plus Nb formula, and a titanium-only heat made to EN 1.4521 will not always pass.

## Mechanical properties, annealed

| Property | ASTM A240 minimum (Cleveland-Cliffs, sheet and strip) | Typical (Cleveland-Cliffs) | EN 10028-7 hot-rolled plate (Virgamet) |
|---|---|---|---|
| Tensile strength Rm | 414 MPa (60 ksi) | 515 MPa (75 ksi) | 420 to 620 MPa, longitudinal |
| 0.2% proof strength Rp0.2 | 276 MPa (40 ksi) | 360 MPa (52 ksi) | 280 MPa min, longitudinal |
| Elongation | 27% min in 50.8 mm | 30% | 20% min |
| Hardness | B90 max | B85 | 185 HB max |

AZoM lists grade 444 at 415 MPa tensile, 275 MPa yield, 20% elongation and 95 HRB. ModulusMetal gives wider annealed ranges of 400 to 640 MPa tensile, 275 to 350 MPa yield and 20 to 40% elongation. What a given forging achieves depends on section size and final anneal; measured values appear on the EN 10204 3.1 certificate for the heat.

### Minimum yield strength against temperature, 1.4521 (Virgamet)

| Temperature, C | 50 | 100 | 150 | 200 | 250 | 300 | 350 | 400 |
|---|---|---|---|---|---|---|---|---|
| Re min, MPa | 294 | 250 | 240 | 230 | 220 | 210 | 205 | 200 |

## Physical properties at room temperature

| Property | Cleveland-Cliffs (Type 444) | Metalcor / Virgamet (1.4521) |
|---|---|---|
| Density | 7.75 g/cm3 (0.28 lb/in3) | 7.7 to 7.73 g/cm3 |
| Thermal conductivity | 26.8 W/m.K at 100 C | 23 W/m.K |
| Coefficient of thermal expansion | 11.0 um/m.K, 0 to 100 C | 10.4 x 10-6 /K |
| Specific heat | 0.427 kJ/kg.K | 0.43 kJ/kg.K |
| Electrical resistivity | 57 uOhm.cm | 0.8 Ohm.mm2/m |
| Modulus of elasticity | not stated | 220 GPa (Metalcor); 195 to 205 GPa (ModulusMetal) |

## Forging and heat treatment

Parameters used at our Jiangyin works, taken from the published 1.4521 processing data (Virgamet).

| Operation | Parameters |
|---|---|
| Forging | 1050 down to 750 C, then water, air or gas cooling |
| Hot rolling | 1050 down to 750 C, then water, air or gas cooling |
| Annealing | 750 to 900 C, air or gas cooling; furnace cooling only in special cases |
| Hardening | Not applicable, ferritic grade |

475 C embrittlement: ferritic stainless steels lose toughness if held in, or cooled slowly through, roughly 315 to 540 C. This is a different mechanism from sigma-phase embrittlement, which occurs at higher temperatures. Cooling after forging and after annealing must be brisk through that band, and it also caps practical continuous service temperature well below the oxidation limit of the grade.

### Welding

Cleveland-Cliffs describes the ferritic class as generally weldable by common fusion and resistance methods, but states that Type 444 welds less readily than Type 409 because of its higher chromium plus molybdenum and niobium content, calling for low heat input, few discontinuities and occasional pre-warming before forming. AWS E/ER 316L is the filler normally specified; Metalcor lists 1.4430. Virgamet places the steel in ISO welding group 7.1, with good weldability in small cross-sections, limited weldability in larger ones, and preheating recommended.

## Corrosion resistance compared with 304 and 316

| Criterion | AISI 444, ferritic | Type 304 / 316, austenitic |
|---|---|---|
| General corrosion | Equal to Type 304 in many environments; Metalcor rates it equal to 1.4401 and 1.4404 | Baseline |
| Chloride stress corrosion cracking | Better than both 304 and 316; SSINA lists ferritics including 444 as very resistant | Susceptible |
| Pitting and crevice | Better than most ferritics and some austenitics, PREN about 25 | 304 lower, 316 comparable |
| Thermal expansion | Lower | Higher |
| Thermal conductivity | Better | Lower |
| Nickel content | 1% max | 8 to 14% |
| Magnetic | Yes | No, in the annealed condition |
| Weldability and low-temperature toughness | More restricted | Generally better |

Cleveland-Cliffs reports good corrosion resistance in moderately severe environments, including chlorides and the organic acids found in foods and beverages, plus satisfactory resistance to dilute sulfuric acid and to highly concentrated sodium hydroxide. Virgamet notes underwater use is acceptable provided chloride concentration stays below about 200 ppm, with a lower limit in hot water or where the design is conservative, and gives a critical pitting temperature below 10 C. AISI 444 is therefore not a seawater immersion grade; duplex or 6-Mo alloys suit that duty.

## Typical applications

Cleveland-Cliffs lists food processing, brewery and wine-making equipment, hot-water tanks, heat exchanger tubing and automotive components, and notes that oxidation and creep resistance at elevated temperature make Type 444 a preferred material in demanding automotive exhaust work. Metalcor adds cold-heading parts and heat exchanger tubes. Virgamet lists bolts, nuts, hot water tanks and chimney ducts.

In forged form the grade is most often supplied for heat exchanger tubesheets and shell flanges, hot water and brewing vessel parts, pump and valve bodies in chloride-bearing water, and shafts and sleeves on jobs where chloride stress corrosion cracking has already caused failures in 304 or 316.

## Forged products supplied

All items are open-die forged to the customer's drawing. There is no fixed size list; send the drawing or a dimensioned sketch with the quantity and the governing standard.

| Category | Items |
|---|---|
| Forged bars | Round bars, rods, square bars, rectangular and flat bars, hexagonal bars, step shafts |
| Hollow sections | Hollow bars, sleeves, bushes and bushings, forged pipes and tubes, barrels, casings, shells, cylinders, hubs, housings |
| Rings | Forged rings, seamless rolled rings, ring flanges, retaining rings |
| Flat products | Discs, disks, blocks, forged plates, tubesheets |
| Other | Forged blanks and near-net shapes, rough-machined and finish-machined parts |

Standard documentation is a chemical analysis and mechanical test report to EN 10204 3.1. Ultrasonic testing, PMI, dye penetrant, intergranular corrosion testing to ASTM A262, hardness mapping and third-party witness inspection are available on request and should be stated at enquiry stage.

Specification warning: ASTM A182 grade F44 is not AISI 444. F44 is the 6-Mo super-austenitic grade UNS S31254. Where a piping specification calls for F44, confirm which material is intended before ordering. Both are supplied, but they are different alloys at very different prices.

## Frequently asked questions

**What is AISI 444 stainless steel?**
A low-carbon, low-nitrogen stabilised ferritic stainless steel with about 18% chromium and 2% molybdenum, designated UNS S44400, JIS SUS444 and EN 1.4521 X2CrMoTi18-2. Cleveland-Cliffs describes it as equivalent to Type 304 in many corrosion environments, with pitting and crevice corrosion resistance better than most ferritic stainless steels and some austenitic grades. It is magnetic and cannot be hardened by heat treatment.

**Is AISI 444 better than 316 stainless steel?**
It depends on the failure mode. Cleveland-Cliffs states Type 444 has chloride stress corrosion cracking resistance better than Type 304 and Type 316, and Metalcor rates 1.4521 corrosion resistance as equal to 1.4401 and 1.4404. Against that, 444 is ferritic: toughness is lower, minimum service temperature is limited, and Cleveland-Cliffs rates weldability below even Type 409. For chloride SCC problems in hot water and heat exchanger service, 444 is often the better engineering answer. For cryogenic duty or heavily welded fabrication, 316L still wins.

**At what temperature is AISI 444 forged?**
From 1050 C down to a 750 C finish, followed by water, air or gas cooling, then annealing at 750 to 900 C with air or gas cooling. Cooling must be brisk through about 315 to 540 C to avoid 475 C embrittlement.

**Can AISI 444 be welded?**
Yes, by common fusion and resistance methods, with low heat input to avoid brittle weld fractures. AWS E/ER 316L is the usual filler; Metalcor lists 1.4430. Preheating is recommended for larger cross-sections.

**Which standards cover AISI 444?**
ASTM A240 for plate, sheet and strip; ASTM A268 for tubing; EN 10028-7 for 1.4521 flat products for pressure purposes. Forgings are normally ordered to A240 or EN 10028-7 chemistry with mechanical properties agreed on the purchase order, because no dedicated ASTM forging specification is in wide use for this grade.

**Can Jiangyin Jiangnan Metal supply small quantities?**
Yes. Single prototype rings and discs are run alongside production batches. Send the drawing to sales@steelforgepieces.com for feasibility, weight and lead time, usually answered within one working day.

## Related grades

PH13-8Mo, 15-5PH, 17-7PH, Incoloy 825, Incoloy 800H, Inconel 690, Inconel 625, all supplied as open-die forgings.

## Contact

Jiangyin Jiangnan Metal Co., Ltd., open-die forging factory
No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
Tel +86-189-2135-9659
Email sales@steelforgepieces.com
Enquiries answered within 24 hours, Monday to Saturday, China Standard Time (UTC+8).

References: Cleveland-Cliffs, 444 Stainless Steel product data, May 2021; Metalcor datasheet 1.4521; Virgamet 1.4521 / X2CrMoTi18-2 technical page; AZoM, Grade 444 (UNS S44400); ModulusMetal AISI 444 data sheet; SSINA guidance on chloride stress corrosion cracking.

Compiled by the technical sales department, Jiangyin Jiangnan Metal Co., Ltd. Figures are for guidance. Certified values for an order are those printed on the EN 10204 3.1 certificate supplied with the goods.