# AISI 309H Forgings (UNS S30909 / 1.4833)

**Source:** https://www.steelforgepieces.com/Stainless-Steel/AISI-309H.html
**Supplier:** Jiangyin Jiangnan Metal Co., Ltd., open-die forging factory
**Address:** No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
**Phone / WhatsApp:** +86-189-2135-9659
**Email:** sales@steelforgepieces.com
**Reviewed:** 30 September 2026

## Summary

AISI 309H (UNS S30909) is the high-carbon version of the 309 family of austenitic heat-resistant
stainless steels: 22.0 to 24.0 % chromium, 12.0 to 15.0 % nickel, carbon 0.04 to 0.10 %. The carbon
range, against 0.08 % maximum for 309S, gives the grade its creep strength above roughly 1000 F
(537 C). Oxidation resistance reaches about 1900 F (1038 C) in non-cyclic service and falls to near
1850 F (1010 C) with frequent thermal cycling. The grade is used for hot service, not wet corrosive
duty.

Jiangyin Jiangnan Metal Co., Ltd. forges 309H to customer drawing: seamless rolled rings, flanges,
shafts, discs, bars, hollow sections and tube sheets, solution annealed, with EN 10204 3.1 or 3.2
certification.

## What 309H is, and what it is not

The 309 grades differ only in carbon. Plain 309 permits up to 0.20 % C, 309S is capped at 0.08 % C
for easier fabrication and better as-welded corrosion behaviour, 309H is held at 0.04 to 0.10 % C for
creep strength. One heat often meets both 309S and 309H limits, so dual certification is common.

309H is not a niobium-stabilised grade; niobium stabilisation belongs to 347 and X7CrNiNb18-10, which
are different materials. 309H is also not an aqueous corrosion grade: the carbon that helps creep
works against wet corrosion resistance, and intergranular attack can follow long exposure at
temperature. Its 23 % chromium still makes it more corrosion resistant than most other heat-resistant
alloys.

## Chemical composition, weight %

| Element | A182 F309H (forgings) | A240 309H (plate) |
|---|---|---|
| Carbon, C | 0.04 to 0.10 | 0.04 to 0.10 |
| Chromium, Cr | 22.0 to 24.0 | 22.0 to 24.0 |
| Nickel, Ni | 12.0 to 15.0 | 12.0 to 15.0 |
| Manganese, Mn | 2.00 max | 2.00 max |
| Silicon, Si | 1.00 max | 0.75 max |
| Phosphorus, P | 0.045 max | 0.045 max |
| Sulphur, S | 0.030 max | 0.030 max |
| Iron, Fe | Balance | Balance |

Silicon differs between the two specifications. Order to one specification and name it on the drawing.

## Mechanical properties, ASTM A182 F309H

| Property | Imperial | Metric |
|---|---|---|
| Tensile strength, min | 75 ksi | 515 MPa |
| Yield strength, 0.2 % offset, min | 30 ksi | 205 MPa |
| Elongation in 2 in. (50 mm) or 4D, min | 30 % | 30 % |
| Reduction of area, min | 50 % | 50 % |

Specification minima, not typical results. Annealed product in this family commonly tests nearer
586 MPa tensile, 310 MPa yield, 50 % elongation, hardness up to about 202 HBN.

## Physical properties

| Property | Value |
|---|---|
| Density | 7.89 g/cm3 (0.285 lb/in3) |
| Modulus of elasticity | 193 GPa (28.5 x 10^6 psi) |
| Melting range | 1480 to 1530 C (2500 to 2590 F) |
| Specific heat, 0 to 100 C | 502 J/kg.K |
| Thermal conductivity at 100 C | 15.6 W/m.K |
| Electrical resistivity at 20 C | 78 microhm.cm |

## Creep data, typical, MPa

| Temperature | Creep strain 1 000 h | 10 000 h | 100 000 h | Rupture 1 000 h | 10 000 h | 100 000 h |
|---|---|---|---|---|---|---|
| 600 C / 1112 F | 120 | 80 | 40 | 190 | 120 | 65 |
| 700 C / 1292 F | 50 | 25 | 20 | 75 | 36 | 16 |
| 800 C / 1472 F | 20 | 10 | 8 | 35 | 18 | 7.5 |
| 900 C / 1652 F | 8 | 4 | 3 | 15 | 8.5 | 3 |
| 1000 C / 1832 F | 4 | 2.5 | 1.5 | 8 | 4 | 1.5 |

## Oxidation limits in air

| Condition | Limit |
|---|---|
| Non-cyclic service | 1038 C (1900 F) |
| Frequent thermal cycling | approx. 1010 C (1850 F) |

Sulphur-bearing, nitriding and carburising atmospheres reduce these limits. The alloy is not
recommended for strongly carburising service; Alloy 600 or Alloy 800H suit those conditions better.

## Heat treatment, forging, machining

- Solution anneal: 1100 to 1150 C (2012 to 2102 F), rapid cooling. Same cycle restores toughness
  after work or service in the 650 to 950 C sigma-phase band.
- Hot forging: 950 to 1200 C (1742 to 2192 F), finish anneal 1000 to 1150 C with rapid quench.
- Machining: work-hardens rapidly, so rigid set-ups, positive feeds, sharp tools, generous coolant.
- Welding: TIG, plasma, MIG, SMAW, SAW, FCAW. Where as-welded corrosion resistance matters, specify
  309S instead.

## Equivalent designations

| System | Designation |
|---|---|
| AISI / trade name | 309H, AISI 309H, Alloy 309H |
| UNS | S30909 |
| Forgings | ASTM A182 F309H, ASME SA182 F309H |
| Plate | ASTM A240 309H, ASME SA240 309H |
| EN / Werkstoff, family | 1.4833, X12CrNi23-13 |

Guidance only. EN 1.4833 covers the 309 family but its chemistry limits are not identical to the ASTM
grades.

## Forged products available in 309H

Seamless rolled rings and retaining rings; weld neck, slip-on, blind and special flanges plus flange
blanks; shafts, step shafts, eccentric shafts, spindles; discs, upset discs and machined blanks;
forged round bar; sleeves, bushings and hollow bar; forged tube blanks and tube sheets; valve bodies,
bonnets, seat rings, stems and blocks; nozzles, manifolds, forging rolls and custom open-die shapes.

Parts are forged to customer drawing. Send the drawing or the finished dimensions and weight for
confirmation of feasibility, forging weight and price.

## Typical applications

Furnace burners, doors, fans, piping and recuperators; fluidised-bed grids, piping and wind boxes;
muffles, retorts, annealing boxes, salt pots and walking beams; catalytic recovery systems in
refining; pulverised-coal burners and tube hangers in power generation; paper-mill equipment;
incinerators, rotary kilns and calciners.

## Melting, testing, certification

- Melting: EAF plus VOD, ESR remelt on request.
- Delivery condition: solution annealed, as-forged or rough machined to drawing.
- Ultrasonic testing to EN 10228-3, SEP 1921 or ASTM A388 as ordered.
- Further NDT on request: PT, MT, chemical analysis, mechanical testing, grain size.
- Certification: EN 10204 3.1, or EN 10204 3.2 witnessed by a third party.

## Questions

**309H against 309S?** Carbon only: 0.08 % max for 309S, 0.04 to 0.10 % for 309H. 309H has higher
creep strength, 309S fabricates and welds more easily.

**309H against 310S?** 310S carries roughly 25 % Cr and 20 % Ni against 23 % Cr and 13.5 % Ni, so it
holds up better at the top of the temperature range. 309H is chosen for creep strength at moderate to
high temperature with lower nickel content.

**Maximum temperature?** About 1038 C (1900 F) non-cyclic, near 1010 C (1850 F) with frequent cycling,
lower in sulphur-bearing, nitriding or carburising gas.

**Magnetic?** Essentially non-magnetic as solution annealed; cold work can raise a slight response.

**Sizes?** Depends on press and ring-mill capacity for the shape. Send the drawing or finished
dimensions and weight for confirmation.

**Ordering?** Send drawing or dimensions, governing specification, quantity, NDT and certification
level, delivery destination to sales@steelforgepieces.com or +86-189-2135-9659.

## References

- Sandmeyer Steel Company, specification sheet for Alloy 309 / 309S / 309H, UNS S30900, S30908,
  S30909, W.Nr. 1.4833.
- Boltport, ASTM A182 F309H composition and mechanical properties.
- ASTM A182 / ASME SA182 and ASTM A240 / ASME SA240, current editions.

Figures support material selection and are not a warranty of fitness for a particular purpose.