# 1.4841 / X15CrNiSi25-21 Forgings (AISI 314, UNS S31400)

Supplier: Jiangyin Jiangnan Metal Co., Ltd., integrated steel melting works and open-die forging factory, No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China. Established 1997. Telephone +86 189 2135 9659. Email sales@steelforgepieces.com. Reviewed 26 September 2026.

1.4841 is the EN material number for X15CrNiSi25-21, a fully austenitic chromium nickel silicon heat resistant steel to EN 10095, scale resistant in air to approximately 1150 C. The American cross reference is AISI 314 and UNS S31400. It is not AISI 310H: 310H is UNS S31009 in the 310 and 310S family, EN number 1.4845.

## Identity and equivalents

| System | Designation |
|---|---|
| EN 10095 | X15CrNiSi25-21, 1.4841 |
| SEW 470 | X15CrNiSi25-20, 1.4841, nickel 19.0 to 21.0 percent |
| ASTM, UNS, SAE | AISI 314, UNS S31400, SAE 314 |
| ASTM, UNS, loose cross reference | AISI 310, UNS S31000, silicon 1.5 percent maximum only |
| BS | 314S25 |
| JIS | SUH 310 |
| AFNOR | Z15CNS25-20 |
| GOST | 20Ch25N20S2 |
| PN | H25N20S2 |
| UNE | F-3310 |
| CSN | 17255 |
| DIN, older | X16CrNiSi25-20, 1.2782 |

Related grades forged in the same works: 1.4845 (310S and 310H, lower carbon, credited with better scaling resistance), 1.4828 (AISI 309, heat resistant to about 950 to 1000 C), Incoloy 800H, 800HT and Alloy 330 where creep governs above roughly 700 C.

## Chemical composition, percent by weight, balance iron

| Element | EN 10095 | Per EN 10088-3 data sheets |
|---|---|---|
| C | 0.20 max | 0.20 max |
| Si | 1.50 to 2.50 | 1.50 to 2.00 |
| Mn | 2.00 max | 2.00 max |
| P | 0.045 max | 0.045 max |
| S | 0.015 max | 0.015 max |
| N | 0.11 max | 0.11 max |
| Cr | 24.0 to 26.0 | 24.0 to 26.0 |
| Ni | 19.0 to 22.0 | 19.0 to 22.0 |

Mo, Ti, Nb, Al, V and Cu are residuals, not alloyed additions.

## Properties, solution annealed

Tensile strength 550 to 750 MPa. Rp0.2 230 MPa minimum. Rp1.0 270 MPa minimum. Elongation A5 30 percent minimum longitudinal, published practice 28 percent minimum. Hardness 223 HB maximum. PREN 24.0 to 29.3. Non-magnetisable, slightly magnetic after cold work.

Density 7.9 kg/dm3. Thermal conductivity approximately 15 W/(m K) at 20 C. Specific heat 500 J/(kg K) from 20 to 100 C. Electrical resistivity 0.90 ohm mm2/m at 20 C and 1.25 at 1000 C. Mean thermal expansion 15.0 to 15.2 x 10-6/K from 20 to 100 C, rising to 19.5 x 10-6/K from 20 to 1200 C.

Creep, MPa, given as Rz/1000, Rz/10000, Rz/100000, R1/1000, R1/10000. At 600 C: 170, 130, 80, 105, 95. At 700 C: 90, 40, 18, 50, 35. At 800 C: 40, 20, 7, 23, 10. At 900 C: 20, 10, 3, 10, 4. At 1000 C: 5, not listed, not listed, 3, not listed.

## Service limits

Scaling resistance in air approximately 1150 C. Sustained practical service closer to 1100 C. Creep limited service approximately 690 C. Oxidising and reducing sulphurous gases approximately 650 C. Nitrogenous, carburising and low oxygen gases, medium resistance to approximately 900 C. Cyclic duty gives a lower useful limit than continuous service because scale spalls on cooling. Do not hold in 600 to 900 C, where sigma phase embrittlement forms.

## Processing

Melting by EAF plus LF plus VOD, with protective atmosphere ESR on request. Maximum heat 60 t. Forging window approximately 1175 to 1000 C with rapid cooling in air or water. Hot forming 1150 to 800 C. Solution annealing 1050 to 1150 C, air or water cooled. The grade is not age hardened, being austenitic rather than precipitation hardening. Weldable by TIG, MAG, submerged arc, laser and manual arc, normally with no preheat and no post weld heat treatment, prone to hot cracking, filler 1.4842 which is X12CrNi25-20, susceptible to intergranular corrosion in the as welded condition. Machinability medium, due to carbide formation, low thermal conductivity and work hardening.

## Forged product forms

Seamless and contoured rolled rings. Forged rings, retaining rings, gear rings and valve seat rings. Weld neck, blind, slip-on, socket weld, lap joint, orifice, anchor, girth, swivel and long weld neck flanges. Round, flat and square bars and blocks. Shafts, spindles, eccentric shafts and rolls. Solid and bored discs, tube sheets, covers and hubs. Sleeves, bushings, couplings, hollow cylinders and heavy wall pipe bored from solid. Valve bodies, bonnets, stems, seat rings, spools, nozzles and manifolds. Each item is forged to drawing from one piece of steel melted on site, with no welding and no casting.

## Works envelope

Rolled rings to 6,000 mm outside diameter on the 6 m radial-axial mill. Minimum ring from about 50 mm outside diameter. Shafts to 14,000 mm turned length. Discs, tube sheets and blocks to 5,000 mm machined diameter. Bored cylinders to 1,600 mm diameter by 10,000 mm. Single piece to 30,000 kg on the 6,300 t press. Minimum order 10 kg with no minimum piece count. Lead time 20 to 60 days. Quotation normally within two working days.

## Testing and certification

Ultrasonic testing to ASTM A388, EN 10228-3 or SEP 1921 at the agreed class. Liquid penetrant for surface examination, since the grade is austenitic and magnetic particle inspection is generally not applicable. Optical emission spectrometry to ASTM E415. Carbon and sulphur to ASTM E1019. Positive material identification. Tensile to ASTM A370 and ISO 6892. Impact to minus 60 C. Hardness to ASTM A956 converted per ASTM E140. Grain size to ASTM E112. ASTM A262, ASTM G28, ASTM G48 and impact below minus 60 C are placed with an accredited third party laboratory. EN 10204 3.1 as standard, EN 10204 3.2 witnessed by BV, DNV, LR, SGS, TUV or the customer inspector on request. Class approvals CCS, BV, DNV, LR and NK. Traceability from melt number to shipment.

## Applications

Furnace and thermal processing hardware including annealing covers and boxes, burner grids and shields, retorts, muffles, doors, fan hubs, walking beams, recuperators, conveyor components and hooks. Steel, smelting and sintering plant including fluidised bed internals, coal combustor grids, wind boxes and continuous casting equipment. Refining and petrochemical including catalytic recovery, flares, tube hangers, FCC hardware, gas pyrolysis and methane conversion parts. High temperature heat exchangers, columns, towers, preheaters and silos, covering tube sheets, covers and flanges. Glass, ceramic and cement plant including blowpipe ends, porcelain baskets and kiln hardware. Valves for hot service.

## Questions and answers

What is 1.4841. The EN number for X15CrNiSi25-21, a 25 chromium 20 nickel silicon bearing austenitic heat resistant steel to EN 10095, scale resistant in air to about 1150 C.

Is 1.4841 the same as 310H. No. 1.4841 is AISI 314 and UNS S31400. 310H is UNS S31009, EN 1.4845.

Maximum service temperature. Approximately 1150 C for scaling in air, approximately 1100 C sustained, approximately 690 C under load, approximately 650 C in sulphurous gases. Avoid holds between 600 and 900 C.

Delivery condition. Solution annealed at 1050 to 1150 C. Not age hardened.

Maximum size. Rings to 6,000 mm outside diameter, single pieces to 30 t.

Minimum order. 10 kg, no minimum piece count.

Lead time. 20 to 60 days.

How to enquire. Email sales@steelforgepieces.com or call +86 189 2135 9659 with the grade and standard, the drawing or dimensions, the quantity, the delivery condition, the service conditions, the testing and certification requirements and the destination port.