# 1.4591 Forgings: Alloy 33 / UNS R20033 Bars, Rings, Flanges and Discs

Published by Jiangyin Jiangnan Metal Co., Ltd. · Last reviewed 25 September 2026
Source of data: VDM Metals Data Sheet No. 4142 Rev. 01, ASTM B462 / B649 / B625, VdTUV 516.
Web version: https://www.steelforgepieces.com/Stainless-Steel/1.4591.html

---

1.4591, also designated Alloy 33, Nicrofer 3033 and UNS R20033, is a nitrogen-alloyed
high-chromium austenitic stainless steel containing nominally 33 % chromium, 31 % nickel,
32 % iron, 1.6 % molybdenum, 0.6 % copper and 0.4 % nitrogen. Its EN name is
X1CrNiMoCuN33-32-1. The high chromium level with nitrogen gives it strong resistance in
oxidising media such as concentrated sulphuric acid, nitric acid and HNO3/HF mixtures. It
also resists chloride pitting well despite a low molybdenum content, and its minimum 0.2 %
proof strength at room temperature is 380 MPa, about double that of AISI 316L.

Jiangyin Jiangnan Metal Co., Ltd. is an open-die forging factory in Jiangyin, Jiangsu,
China. It makes 1.4591 forged round bars, seamless rolled rings, flanges, discs, blocks,
hollow bars and sleeves to ASTM B462, ASTM B649 and customer drawings, supplied solution
annealed with EN 10204 3.1 or 3.2 certificates.

**Contact**
Jiangyin Jiangnan Metal Co., Ltd., Open-Die Forging Factory
No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
Tel 0086-189-2135-9659 · Email sales@steelforgepieces.com

---

## Key data

| Item | Value |
|---|---|
| EN / Werkstoff number | 1.4591 |
| EN steel name | X1CrNiMoCuN33-32-1 |
| UNS number | R20033 |
| Trade names | Alloy 33, Nicrofer 3033 |
| Type | Austenitic, nitrogen-alloyed |
| Rp0.2 minimum at 20 °C | 380 MPa / 55.1 ksi |
| Rm at 20 °C | 720-920 MPa |
| Elongation A minimum | 40 % |
| PREN (16×N formula) | 44.7 |
| Density | 7.9 g/cm³ |
| Solution anneal | 1100-1150 °C, water quench |
| ASME service range | -196 °C to +450 °C |

---

## What is 1.4591 (Alloy 33 / UNS R20033)?

1.4591 is a chromium-based austenitic stainless steel introduced in 1995 for service
conditions that defeat ordinary austenitic and super-austenitic grades: hot concentrated
sulphuric acid, nitric acid, mixed acids and chloride-bearing process streams. Instead of
relying on molybdenum, it relies on a very high chromium level of about 33 %, backed by
roughly 0.4 % nitrogen and small additions of molybdenum and copper.

Three things define the grade:

- **Chromium-driven passivity.** At 33 % Cr the passive film stays stable in strongly
  oxidising acids that attack molybdenum-rich alloys.
- **Nitrogen strengthening.** About 0.4 % nitrogen, stabilised by 31 % nickel, holds the
  structure fully austenitic, raises minimum proof strength to 380 MPa and slows
  sigma-phase precipitation.
- **Copper and molybdenum additions.** About 0.6 % Cu and 1.6 % Mo help passivation in
  sulphuric acid and improve behaviour in phosphoric acid.

For a forging shop and for the end user this means three practical things: a high
work-hardening rate that changes machining and cold-forming parameters, a narrow
hot-working window, and a compulsory solution anneal with rapid quench after forging to
restore corrosion performance.

On naming: 1.4591, Alloy 33, Nicrofer 3033, X1CrNiMoCuN33-32-1 and UNS R20033 are the same
material. Some distributors quote UNS N08033; ASTM specifications use R20033.

---

## Designations, equivalents and standards

ASTM classifies 1.4591 as a chromium-nickel-iron-nitrogen low-carbon alloy. It appears in
the same specifications as super-austenitic grades such as 1.4562 (Alloy 31, UNS N08031)
and 1.4529 (UNS N08926).

### Table 1. Designations of 1.4591 / Alloy 33

| System | Designation |
|---|---|
| EN / Werkstoff number | 1.4591 |
| EN steel name | X1CrNiMoCuN33-32-1 |
| UNS | R20033 |
| Trade names | Alloy 33, Nicrofer 3033 |
| Welding consumable | AWS A5.9 ER33-31, ISO 14343-A S Z 33 32 1 Cu N L |
| GB/T (China) | No direct national equivalent; supplied to EN or ASTM designation |

### Table 2. Product-form standards for 1.4591

| Product form | ASTM | ASME | DIN / VdTUV / other |
|---|---|---|---|
| Forged flanges, fittings, valves and parts | B462 | SB-462 | VdTUV 516 |
| Bar, rod and wire | B649 | SB-649 | VdTUV 516 |
| Plate, sheet and strip | B625 | SB-625 | EN 10029, SEW 400, VdTUV 516 |
| Pressure-vessel approval | ASME, from -196 °C to 450 °C | SB-462 / SB-649 / SB-625 | VdTUV 516 |

For forged components the governing specification is normally ASTM B462, which covers
forged or rolled pipe flanges, forged fittings, valves and parts in UNS R20033 for
corrosive high-temperature service.

---

## Chemical composition of 1.4591 (Alloy 33)

Iron is the balance, typically about 32 %.

### Table 3. Chemical composition, weight %

| Element | Symbol | Min. | Max. | Nominal |
|---|---|---:|---:|---:|
| Chromium | Cr | 31.0 | 35.0 | 33 |
| Nickel | Ni | 30.0 | 33.0 | 31 |
| Iron | Fe | Balance | Balance | 32 (bal.) |
| Molybdenum | Mo | 0.5 | 2.0 | 1.6 |
| Nitrogen | N | 0.35 | 0.6 | 0.4 |
| Copper | Cu | 0.3 | 1.2 | 0.6 |
| Manganese | Mn | - | 2.0 | - |
| Silicon | Si | - | 0.5 | - |
| Carbon | C | - | 0.015 | 0.010 typ. |
| Phosphorus | P | - | 0.020 | - |
| Sulphur | S | - | 0.010 | - |

Carbon is held below 0.015 % to suppress chromium-carbide precipitation. Ageing for up to
8 hours between 600 °C and 1000 °C does not sensitise the alloy when tested in boiling
azeotropic nitric acid (Huey test), which leaves useful margin during welding and forging.

---

## Mechanical properties of 1.4591

Values apply to solution-annealed material, for longitudinal and transverse specimens.

### Table 4. Minimum mechanical properties at room temperature (20 °C / 68 °F)

| Product form | Dimension | Rp0.2 | Rp1.0 | Rm | A |
|---|---|---:|---:|---:|---:|
| Sheet and plate (ASTM B625) | ≤ 50 mm (1.97 in) | ≥ 380 MPa (55.1 ksi) | ≥ 420 MPa (60.9 ksi) | 720-920 MPa (104-133 ksi) | ≥ 40 % |
| Bar and rod (ASTM B649) | ≤ 150 mm (5.91 in) | ≥ 380 MPa (55.1 ksi) | ≥ 420 MPa (60.9 ksi) | 720-920 MPa (104-133 ksi) | ≥ 40 % |

### Table 5. Minimum proof strength at elevated temperature (VdTUV 516)

| Temperature | Rp0.2 | Rp1.0 |
|---:|---:|---:|
| 20 °C (68 °F) | 380 MPa | 420 MPa |
| 100 °C (212 °F) | 320 MPa | 350 MPa |
| 200 °C (392 °F) | 270 MPa | 300 MPa |
| 300 °C (572 °F) | 240 MPa | 270 MPa |
| 400 °C (752 °F) | 220 MPa | 250 MPa |
| 500 °C (932 °F) | 210 MPa | 240 MPa |

### Table 6. Hardness and impact toughness

| Property | Condition | Value |
|---|---|---:|
| Brinell hardness | Sheet ≤ 50 mm, strip ≤ 3 mm, bar ≤ 150 mm | ≤ 240 HBW |
| ISO-V notch impact energy, 20 °C | Sheet | ≥ 150 J (111 ft·lbf) |
| ISO-V notch impact energy, 20 °C | Bar and forgings | ≥ 120 J |

Weld metal deposited with matching filler reaches mechanical properties and ISO-V impact
toughness close to wrought plate, with no measured loss of toughness in the heat-affected
zone. That is why 1.4591 is accepted for welded pressure equipment.

---

## Physical properties of 1.4591

### Table 7. Physical properties at 20 °C (68 °F)

| Property | Metric | Imperial |
|---|---:|---:|
| Density | 7.9 g/cm³ | 493 lb/ft³ (0.285 lb/in³) |
| Melting range | 1330-1370 °C | 2430-2498 °F |
| Relative magnetic permeability | 1.01 | 1.01 |
| Modulus of elasticity | 195 GPa | 28.3 × 10³ ksi |
| Specific heat capacity (25 °C) | 446 J/(kg·K) | 0.107 Btu/(lb·°F) |
| Thermal conductivity | 13.4 W/(m·K) | 7.74 Btu·in/(ft²·h·°F) |
| Electrical resistivity | 104 µΩ·cm | 104 µΩ·cm |
| Crystal structure | Face-centred cubic, fully austenitic | Face-centred cubic, fully austenitic |

### Table 8. Property variation with temperature

| T | Specific heat J/(kg·K) | Thermal cond. W/(m·K) | Resistivity µΩ·cm | E-modulus GPa | Mean CTE 10⁻⁶/K |
|---:|---:|---:|---:|---:|---:|
| 20 °C | 446 | 13.4 | 104 | 195 | - |
| 100 °C | 466 | 14.6 | 107 | 185 | 14.5 |
| 200 °C | 486 | 16.0 | 109 | 176 | 15.3 |
| 300 °C | 503 | 17.5 | 112 | 170 | 15.3 |
| 400 °C | 520 | 19.0 | 114 | 163 | 15.7 |
| 500 °C | 538 | 20.4 | 116 | 159 | 16.1 |

---

## How corrosion-resistant is 1.4591?

1.4591 was developed for oxidising service. Its 33 % chromium builds a passive film that
holds up in media which dissolve molybdenum-rich nickel alloys, while the nitrogen and the
modest molybdenum content give chloride pitting resistance on a par with 6 % Mo
super-austenitic steels.

### Pitting resistance equivalent number (PREN)

From the nominal analysis of 33 Cr, 1.6 Mo and 0.4 N:

- PREN = %Cr + 3.3 × %Mo + 16 × %N = 33 + 5.28 + 6.4 = **44.7**
- PREN = %Cr + 3.3 × %Mo + 30 × %N = 33 + 5.28 + 12.0 = **50.3**

Both formulas are in use. The 16×N version is the more conservative one and is usually the
one quoted in specifications. A PREN above 40 is normally called for in seawater service,
so 1.4591 clears that bar on either calculation. Recalculate PREN per heat from the mill
test certificate, because chemistry varies inside the specified limits.

### Table 9. Laboratory corrosion rates in selected media

| Medium | Temperature | Corrosion rate |
|---|---:|---:|
| H2SO4 98 % | 100 °C (212 °F) | 0.04 mm/a |
| H2SO4 98 % | 150 °C (302 °F) | 0.08 mm/a |
| H2SO4 98 % | 200 °C (392 °F) | 0.04 mm/a |
| H3PO4 85 % | 100 °C (212 °F) | 0.08 mm/a |
| H3PO4 85 % | 154 °C (309 °F) | 1.07 mm/a |
| NaOH 25 % | 75 °C and boiling (104 °C) | < 0.01 mm/a |
| NaOH 50 % | 75 °C, 100 °C, boiling (156 °C) | < 0.01 mm/a |
| HNO3 12 % | 90 °C (194 °F) | < 0.01 mm/a |
| HNO3 12 % + HF 0.9 % | - | 0.24 mm/a |
| HNO3 32 % + HF 0.4 % | - | 0.27 mm/a |
| HNO3 45 % + HF 0.4 % | - | 0.67 mm/a |
| HNO3 68 % + HF 0.4 % | - | 3.08 mm/a |

Field tests confirm the laboratory picture in flowing 96 to 98.5 % sulphuric acid at 135 to
140 °C and in flowing 99.1 % sulphuric acid at 150 °C, with usable results reported in 96 %
H2SO4 containing nitrosyl additions at 240 °C.

Surface condition decides real performance. Full corrosion resistance is reached only when
the component is clean and metallically bright. Forging scale, grinding burn, embedded iron
and weld heat tint all cut resistance.

---

## Where is 1.4591 used?

### Table 10. Typical applications and matching forged components

| Industry or service | Typical application | Forgings commonly required |
|---|---|---|
| Sulphuric acid production | Heat-recovery and acid distribution systems, acid coolers and piping contaminated with chlorides | Flanges, tubesheets, valve bodies, forged blocks |
| Nitric acid and nuclear fuel reprocessing | Vessels and transport equipment for HNO3/HF mixtures | Rings, flanges, nozzles, hollow bars |
| Seawater and desalination | Seawater piping, condensers and coolers where chloride pitting decides the material | Seamless rolled rings, flanges, pump shafts, sleeves |
| Chlor-alkali | Production and handling of NaOH and KOH up to 70 wt.-% and 170 °C (338 °F) | Flanges, discs, valve internals |
| Fertiliser and urea | Urea solutions from 5 to 90 wt.-% | High-pressure flanges, forged fittings, blocks |
| Pulp and paper | Bleaching and recovery equipment components | Rings, shafts, sleeves |
| PTA plants | Vessels and piping in purified terephthalic acid service | Flanges, forged fittings, discs |

---

## How is 1.4591 forged and heat treated?

1.4591 is a wrought alloy that takes open-die forging and ring rolling well, but the
process window is tighter than for standard austenitic stainless steels.

**Step 1. Cleanliness before heating.** The billet must be free of sulphur, phosphorus,
lead and other low-melting metals before it goes in the furnace. These embrittle 1.4591 at
forging temperature and are present in marking paints, temperature-indicating crayons,
greases, oils and fuels. Natural gas below 0.1 wt.-% S, fuel oil below 0.5 wt.-% S.
Electric furnaces are preferred.

**Step 2. Furnace atmosphere.** Hold the atmosphere neutral to slightly oxidising and do
not let it swing between oxidising and reducing. Flame must not touch the workpiece.

**Step 3. Hot forging.** Charge the billet into a furnace already at temperature, about
1200 °C (2192 °F) maximum, and forge in the range 1200 to 1000 °C (2192 to 1832 °F).
Finishing below 1000 °C risks cracking. Cool quickly after forging, by water quench or as
fast as the part allows.

**Step 4. Solution annealing.** Solution anneal between 1100 and 1150 °C (2012 to 2102 °F),
preferably at 1120 °C (2048 °F), charging into a furnace already at temperature. Soak time
is counted from the moment the section reaches temperature.

### Table 11. Solution-annealing soak time

| Section thickness d | Soak time t | Example |
|---|---|---|
| d < 10 mm | t = d × 3 min/mm | 8 mm gives 24 min |
| d = 10-20 mm | t = 30 min + (d - 10) × 2 min/mm | 16 mm gives 42 min |
| d > 20 mm | t = 50 min + (d - 20) × 1 min/mm | 120 mm gives 150 min |

Over-soaking does far less harm than under-soaking. Quench in water. Rapid air cooling is
acceptable only below about 3 mm section.

**Step 5. Cold forming, where used.** Cold work only from the solution-annealed condition.
1.4591 work-hardens much faster than standard austenitic stainless steels. Interstage
annealing may be needed for heavy work, and any total cold reduction above 15 % must be
followed by a final solution anneal.

---

## Machining, welding and descaling 1.4591

**Machining.** Machine in the solution-annealed condition. Use low cutting speeds, a
moderate feed, and keep the tool engaged at all times. A tool that dwells leaves a hardened
skin the next pass has to cut through. Depth of cut must be enough to get under the
strain-hardened layer. Use plenty of coolant, preferably aqueous.

**Welding.**

- Filler metal: matching consumable to AWS A5.9 ER33-31 or ISO 14343-A S Z 33 32 1 Cu N L
  (UNS R20033).
- Condition: weld only solution-annealed material, free of scale, grease and markings.
  Degrease the seam faces with acetone.
- Heat input: low and controlled. Interpass temperature must not exceed 100 °C.
- Technique: stringer beads, thin passes. The high nitrogen content makes the weld pool
  prone to porosity, and thin beads let it degas.
- Joint geometry: included angles of 60 to 70° for butt welds, root gaps of 1 to 3 mm.
- Shielding: argon, optionally with up to about 5 % hydrogen, and high-purity root
  protection (min. Ar 4.6).
- Heavy sections: from about 20 mm wall thickness the fill passes may be laid with a
  1.4563-type consumable and capped with at least two layers of matching 1.4591 filler.
- Post-weld heat treatment is normally not required.

**Descaling and pickling.** Oxide scale and weld heat tint stick harder on 1.4591 than on
standard stainless steels. Grind with very fine abrasive belts or discs and avoid grinding
burn. Before pickling in nitric and hydrofluoric acid, break up the oxide layer by grit
blasting, fine grinding or a salt-bath pre-treatment. Where the work allows it, brush the
weld while it is still warm.

---

## 1.4591 forged products supplied by Jiangyin Jiangnan Metal

We are an open-die forging factory, not a stockist reselling mill product. 1.4591 is forged
to order from certified billet, solution annealed in our own furnaces, machined to your
drawing where required, and tested before release.

### Table 12. Forged product range and size capability

| Product form | Size range | Notes |
|---|---|---|
| Forged round bar and shafts | Ø 80-1200 mm, length up to 6000 mm | Turned, peeled or black. Step shafts to drawing |
| Square, rectangular, flat and hex bar | Thickness 30-800 mm | Saw-cut to length |
| Seamless rolled rings | OD 200-3500 mm, wall 30-500 mm, height up to 1000 mm | Ring-rolled, rectangular or profiled section |
| Forged flanges | DN 15 to DN 2000, 1/2" to 80", up to Class 2500 | WN, SO, BL, LJ, orifice, special to drawing |
| Discs, blanks and plates | Ø 100-2500 mm, thickness 20-600 mm | Tubesheets, blind discs, cover plates |
| Hollow bars, sleeves, bushings, cylinders | OD 120-1500 mm, ID from 60 mm | Trepanned or expanded, bored and honed on request |
| Blocks, cubes and custom forgings | Up to 8000 kg single piece | Valve bodies, hubs, housings, casings, barrels |

**Delivery condition and machining allowance**

- Standard condition: forged, solution annealed at 1100 to 1150 °C, water quenched,
  descaled.
- Surface: black as forged and descaled, rough machined, or finish machined to drawing
  tolerance.
- Allowance: typically 6 to 12 mm per side on rough-machined parts, agreed per order.
- Marking: hard stamping or low-stress vibro marking with grade, heat number, order number
  and specification, using sulphur-free and chloride-free marking media.

---

## Quality control, testing and certification

### Table 13. Testing and documentation available

| Category | Scope |
|---|---|
| Chemical analysis | Full spectro analysis per heat including N, C and S. PREN calculated per heat on request |
| Mechanical testing | Tensile (Rp0.2, Rp1.0, Rm, A), Brinell hardness, ISO-V notch impact at 20 °C or low temperature |
| Non-destructive testing | Ultrasonic (UT), dye-penetrant (PT), dimensional inspection. Radiography on request |
| Corrosion testing | Intergranular corrosion per ASTM A262 practice C (Huey) or per customer specification |
| Heat-treatment records | Calibrated furnace charts with charge, soak and quench data for every lot |
| Certification | EN 10204 3.1 as standard. EN 10204 3.2 with third-party witness (TUV, BV, SGS, Lloyd's, DNV) on request |
| Third-party inspection | Welcome at any stage. Customer or agency witnessed testing arranged on order |

---

## 1.4591 against other corrosion-resistant grades

Compositions are nominal and PREN uses the 16×N formula.

### Table 14. 1.4591 against common super-austenitic and duplex alternatives

| Grade | UNS | Cr | Ni | Mo | N | PREN | Rp0.2 min | Best suited to |
|---|---|---:|---:|---:|---:|---:|---:|---|
| 1.4591 / Alloy 33 | R20033 | 33 | 31 | 1.6 | 0.4 | 45 | 380 MPa | Hot concentrated H2SO4, HNO3, HNO3/HF, alkalis, seawater |
| 1.4562 / Alloy 31 | N08031 | 27 | 31 | 6.5 | 0.2 | 51 | 276 MPa | Reducing acids, phosphoric acid, mixed chloride service |
| 1.4547 / 254 SMO type | S31254 | 20 | 18 | 6.1 | 0.2 | 43 | 300 MPa | Seawater, chloride pitting, bleach plants |
| 904L / 1.4539 | N08904 | 20 | 25 | 4.3 | - | 34 | 220 MPa | Dilute sulphuric and phosphoric acid |
| Super duplex 2507 | S32750 | 25 | 7 | 3.8 | 0.27 | 42 | 550 MPa | High-strength chloride service, offshore |
| 316L / 1.4404 | S31603 | 17 | 12 | 2.2 | - | 24 | 170 MPa | General chemical and food service |

**How to choose.** Where the main threat is oxidising, meaning concentrated sulphuric acid
at temperature, nitric acid or HNO3/HF mixtures, the 33 % chromium of 1.4591 is what counts
and it will outlast higher-molybdenum alloys. Where the main threat is reducing acid, a
molybdenum-rich grade such as Alloy 31 or a nickel alloy is usually the better answer.
Where chloride pitting is the problem, 1.4591 and the 6 Mo grades are close, but 1.4591
carries about 25 % more proof strength, which can cut wall thickness and forging weight.

---

## Frequently asked questions about 1.4591

**Is 1.4591 the same as Alloy 33 and UNS R20033?**
Yes. 1.4591 is the EN material number, X1CrNiMoCuN33-32-1 is the EN steel name, R20033 is
the UNS number, and Alloy 33 and Nicrofer 3033 are trade names for the same
nitrogen-alloyed high-chromium austenitic stainless steel. Some distributors also quote UNS
N08033. ASTM specifications use R20033.

**Is 1.4591 a stainless steel or a nickel alloy?**
1.4591 is an austenitic stainless steel by composition, since iron is the balance at about
32 %. With 31 % nickel and 33 % chromium it sits at the boundary with the
nickel-iron-chromium alloys, and it is specified in ASTM standards such as B462 and B649
alongside nickel alloys. In practice it is bought and fabricated like a super-austenitic
stainless steel.

**What is the forging temperature range for 1.4591?**
Hot forge 1.4591 between 1200 °C and 1000 °C (2192 to 1832 °F), charging into a furnace
already at temperature, then cool quickly in water or air. Do not finish below 1000 °C. A
solution anneal at 1100 to 1150 °C followed by a water quench is required after forging to
restore full corrosion resistance.

**What is the PREN of 1.4591?**
Using PREN = %Cr + 3.3 × %Mo + 16 × %N and the nominal analysis of 33 Cr, 1.6 Mo and 0.4 N,
the PREN of 1.4591 is 44.7. With the 30 × %N formula it is 50.3. Both are above the value
of 40 normally called for in seawater service. Recalculate PREN from the actual heat
analysis on the mill certificate.

**Can 1.4591 be welded?**
Yes. 1.4591 is welded with a matching filler to AWS A5.9 ER33-31, using low heat input,
stringer beads and an interpass temperature not above 100 °C. Thin beads matter, because
the high nitrogen content makes the weld pool prone to porosity. Post-weld heat treatment
is normally not required, and weld metal toughness matches wrought material.

**What service temperature is 1.4591 approved for?**
1.4591 holds ASME approval for pressure vessels from -196 °C to 450 °C (-320 °F to 842 °F).
Minimum proof strength falls from 380 MPa at 20 °C to 210 MPa at 500 °C.

**Why is 1.4591 harder to machine than 316L?**
Its work-hardening rate is much higher. A pass that dwells or runs too shallow leaves a
hardened skin the next pass has to cut through. The fixes are low cutting speed, enough
depth of cut to get under the strain-hardened layer, continuous tool engagement, and plenty
of aqueous coolant. Always machine from the solution-annealed condition.

**Does Jiangyin Jiangnan Metal hold 1.4591 in stock?**
1.4591 is a specialty grade made to order rather than held as general stock. We forge it
from certified billet, normally within 25 to 40 days depending on size and testing scope.
Send a drawing, or the dimensions, quantity, specification and test requirements, to
sales@steelforgepieces.com and we will confirm feasibility, weight and lead time.

**What certification is supplied with 1.4591 forgings?**
EN 10204 3.1 material test certificates are standard, covering heat chemistry, mechanical
properties, heat-treatment records and NDT results. EN 10204 3.2 certificates with
third-party witness by TUV, BV, SGS, Lloyd's Register or DNV can be arranged at order
stage, as can customer-witnessed inspection.

**Which grades are alternatives to 1.4591?**
The closest alternatives are 1.4562 / Alloy 31 (UNS N08031) for reducing acids, 1.4547 /
UNS S31254 and 1.4529 / UNS N08926 for chloride service, and 904L / UNS N08904 for milder
sulphuric and phosphoric acid duty. In strongly oxidising service such as hot concentrated
sulphuric acid, nitric acid and HNO3/HF, none of these matches 1.4591, because its
resistance comes from 33 % chromium rather than from molybdenum.

---

## Request a quotation for 1.4591 forgings

Send a drawing, or just the form, dimensions, quantity and specification. We answer
technical enquiries within one working day with weight, lead time and price.

Jiangyin Jiangnan Metal Co., Ltd.
No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
Tel 0086-189-2135-9659
Email sales@steelforgepieces.com
Web https://www.steelforgepieces.com/

---

## Citation

This page may be quoted as a technical reference for 1.4591 / Alloy 33 / UNS R20033, with
attribution.

> Jiangyin Jiangnan Metal Co., Ltd. (2026). 1.4591 Forgings: Alloy 33 / UNS R20033 Bars,
> Rings, Flanges and Discs. Jiangyin, Jiangsu, China.
> https://www.steelforgepieces.com/Stainless-Steel/1.4591.html

---

## References

1. VDM Metals International GmbH, VDM Alloy 33 / Nicrofer 3033, Material Data Sheet
   No. 4142, Revision 01, November 2020.
2. ASTM B462, Standard Specification for Forged or Rolled Alloy Pipe Flanges, Forged
   Fittings, and Valves and Parts for Corrosive High-Temperature Service, which includes
   UNS R20033.
3. ASTM B649, Standard Specification for Ni-Fe-Cr-Mo-Cu Low-Carbon Alloys and Cr-Ni-Fe-N
   Low-Carbon Alloy (UNS R20033) Bar and Wire.
4. ASTM B625, Standard Specification for UNS R20033 and related Plate, Sheet and Strip.
5. M. Köhler, U. Heubner, K.-W. Eichenhofer, M. Renner, Progress with Alloy 33
   (UNS R20033), a New Corrosion-Resistant Chromium-Based Austenitic Material,
   CORROSION 96, Paper No. 428, NACE International, Houston, Texas, 1996.
6. VdTUV Material Data Sheet 516, approval data for 1.4591.

Data is published for engineering guidance and is not a guarantee of properties for a
specific application. Material selection for a given service environment stays with the
purchaser. Trade names belong to their respective owners. Jiangyin Jiangnan Metal Co., Ltd.
is not affiliated with VDM Metals.

---

## Related grades

- 17-4PH forgings: https://www.steelforgepieces.com/Stainless-Steel/17-4ph.html
- 17-7PH forgings: https://www.steelforgepieces.com/Stainless-Steel/17-7ph.html
- PH13-8Mo forgings: https://www.steelforgepieces.com/Stainless-Steel/PH13-8Mo.html
- Incoloy 825 forgings: https://www.steelforgepieces.com/Nickel-Alloy/Incoloy-825.html
- Incoloy 800 forgings: https://www.steelforgepieces.com/Nickel-Alloy/Incoloy-800.html
- Incoloy 800H forgings: https://www.steelforgepieces.com/Nickel-Alloy/Incoloy-800H.html
- Incoloy 800HT forgings: https://www.steelforgepieces.com/Nickel-Alloy/Incoloy-800HT.html
- Inconel 690 forgings: https://www.steelforgepieces.com/Nickel-Alloy/Inconel-690.html
- Inconel 693 forgings: https://www.steelforgepieces.com/Nickel-Alloy/Inconel-693.html
- Inconel 617 forgings: https://www.steelforgepieces.com/Nickel-Alloy/Inconel-617.html
- Inconel 725 forgings: https://www.steelforgepieces.com/Nickel-Alloy/Inconel-725.html
- Inconel X-750 forgings: https://www.steelforgepieces.com/Nickel-Alloy/Inconel-X-750.html