# 1.4547 Forgings: UNS S31254 / ASTM A182 F44 Super-Austenitic Stainless Steel

> Source page: https://www.steelforgepieces.com/Stainless-Steel/1.4547.html
> Publisher: Jiangyin Jiangnan Metal Co., Ltd., open-die forging factory, Jiangyin, Jiangsu, China
> Last reviewed: 25 September 2026

Open-die forged rings, seamless rolled rings, flanges, round bars, discs, shafts, sleeves, bushings,
tube sheets and valve components in 1.4547 (X1CrNiMoCuN20-18-7), produced to order by Jiangyin
Jiangnan Metal Co., Ltd.

## Summary

1.4547 is a 6 percent molybdenum, nitrogen-alloyed super-austenitic stainless steel. EN 10088 names it
X1CrNiMoCuN20-18-7, ASTM uses the UNS number S31254, and ASTM A182 lists it as grade F44 for forgings.
The trade name 254 SMO belongs to Outokumpu. Its pitting resistance equivalent number (PREN) runs 42 to
44, which is high enough for seawater, chloride brines and dilute sulphuric acid at temperatures that
would pit 316L or 904L.

Jiangyin Jiangnan Metal Co., Ltd. forges 1.4547 to order at No. 1 Chengxiqiao Road, Zhouzhuang Town,
Jiangyin City, Jiangsu Province, China. Rings, flanges, bars, discs, shafts and tube sheets are made
from ESR-refined billet and supplied solution annealed, ultrasonically tested and certified to
EN 10204 3.1 or 3.2. Enquiries go to 0086-189-2135-9659 or sales@steelforgepieces.com.

| Key fact | Value |
| --- | --- |
| EN designation | 1.4547 |
| UNS number | S31254 |
| Forging specification | ASTM A182 F44 |
| PREN | 42 to 44 |
| Molybdenum | 6.0 to 7.0 % |
| Delivery condition | Solution annealed |

## Equivalent grades and standards

| System or standard | Designation | Applies to |
| --- | --- | --- |
| EN 10088 material number | 1.4547 | All product forms |
| EN 10088 material name | X1CrNiMoCuN20-18-7 | All product forms |
| UNS | S31254 | All product forms |
| ASTM A182 | F44 | Forged flanges, fittings, valves, parts |
| ASTM A276 / A479 | S31254 | Bars and shapes |
| ASTM A240 | S31254 | Plate, sheet, strip |
| EN 10222-5 / EN 10250-4 | 1.4547 | Pressure-purpose and open-die forgings |
| JIS | SUS 312L, commonly cross-referenced | Pipe, plate |
| Trade and generic names | 254 SMO, Alloy 254, 6Mo austenitic | Proprietary or generic |

254 SMO is a registered trademark of Outokumpu. Jiangyin Jiangnan Metal Co., Ltd. supplies material to
the chemical and mechanical requirements of EN 1.4547 and UNS S31254. It is not sold as proprietary
mill-branded product.

## Chemical composition

Mass percent. Single values are maxima. Balance iron.

| Element | EN 10088, 1.4547 | ASTM A182 F44, S31254 |
| --- | --- | --- |
| Carbon (C) | 0.020 max | 0.020 max |
| Silicon (Si) | 0.70 max | 0.80 max |
| Manganese (Mn) | 1.00 max | 1.00 max |
| Phosphorus (P) | 0.030 max | 0.030 max |
| Sulphur (S) | 0.010 max | 0.010 max |
| Chromium (Cr) | 19.50 to 20.50 | 19.50 to 20.50 |
| Nickel (Ni) | 17.50 to 18.50 | 17.50 to 18.50 |
| Molybdenum (Mo) | 6.00 to 7.00 | 6.00 to 6.50 |
| Nitrogen (N) | 0.180 to 0.250 | 0.180 to 0.220 |
| Copper (Cu) | 0.50 to 1.00 | 0.50 to 1.00 |
| Iron (Fe) | Balance | Balance |

### Pitting resistance equivalent number (PREN)

PREN = %Cr + 3.3 x %Mo + 16 x %N.

At the minimum specification limits of 1.4547 (Cr 19.5 %, Mo 6.0 %, N 0.18 %) the result is
19.5 + 19.8 + 2.88 = 42.2. A typical production heat at Cr 20.0 %, Mo 6.1 %, N 0.20 % gives
20.0 + 20.1 + 3.2 = 43.3. Published datasheets therefore quote a band of 42 to 44. 316L sits near 24
and 904L near 34, which is why 1.4547 gets specified where those grades pit.

## Mechanical properties

Solution annealed condition, room temperature.

| Property | ASTM A182 F44, forgings | EN 10088-3, bar up to 160 mm |
| --- | --- | --- |
| Tensile strength Rm | 650 MPa min (94 ksi) | 650 to 850 MPa |
| 0.2 % proof stress Rp0.2 | 300 MPa min (44 ksi) | 300 MPa min |
| 1.0 % proof stress Rp1.0 | Not specified | 340 MPa min |
| Elongation A | 35 % min | 35 % min |
| Reduction of area Z | 50 % min | Not specified |
| Hardness | No limit in ASTM A182 for F44 | 260 HB max, typically 210 to 230 HB |

Charpy V-notch impact testing is not mandatory in either standard. It is available as a supplementary
test, with acceptance to the governing MDS such as NORSOK M-630, or to the purchase specification.

Minimum properties fall as the ruling section increases. State the finished section thickness and the
applicable standard edition on the enquiry so that the correct acceptance values are quoted.

## Physical properties at 20 C

| Property | Value |
| --- | --- |
| Density | 8.0 g/cm3 (0.289 lb/in3) |
| Modulus of elasticity | 195 GPa |
| Thermal conductivity | 14 W/(m K) |
| Specific heat capacity | 500 J/(kg K) |
| Electrical resistivity | 0.85 micro-ohm m |
| Mean thermal expansion, 20 to 100 C | 16.5 x 10-6 /K |
| Magnetic permeability | About 1.0, non-magnetic when annealed |
| Melting range, approximate | 1320 to 1390 C |
| Typical code temperature limit | About 425 C (800 F) |

## Corrosion resistance

Six percent molybdenum, 0.2 percent nitrogen and roughly 0.7 percent copper put 1.4547 close to
nickel-base Alloy 625 in many chloride services, at a lower cost per kilogram.

- Seawater and chloride brines. Resists pitting and crevice attack in ambient natural seawater. Common
  in firewater, seawater cooling and subsea pipework hardware.
- Stress corrosion cracking. The 18 percent nickel content gives much better resistance to chloride SCC
  than the 8 to 10 percent nickel 300-series grades.
- Acids. Handles dilute sulphuric acid, phosphoric acid, organic acids and mixed acids containing
  chlorides over a wider band of concentration and temperature than 316L or 904L.
- Intergranular corrosion. With carbon held to 0.020 percent maximum, 1.4547 is supplied resistant to
  sensitisation. Acceptance is normally shown by ASTM A262 Practice E.
- Limits. Not for hot concentrated sulphuric or hydrochloric acid, and no substitute for nickel alloys
  in strongly reducing media. Prolonged exposure above roughly 500 C risks intermetallic (sigma and chi)
  precipitation and should be avoided.

For offshore procurement, pitting resistance is usually verified by the ASTM G48 Method A ferric
chloride test at 40 C following NORSOK M-630 practice, with acceptance at no pitting under 20x
magnification and weight loss not exceeding 4.0 g/m2.

## How 1.4547 forgings are made

1.4547 is one of the harder austenitic grades to forge. High molybdenum and nitrogen narrow the
hot-working window and raise flow stress well above 316L.

1. Melting. EAF with AOD or VOD refining, then electroslag remelting (ESR) where cleanliness or large
   section size calls for it.
2. Heating. Billet soaked at 1150 to 1200 C with controlled soak time, so intermetallic phases are
   fully dissolved before the first blow.
3. Open-die forging. Upsetting, drawing, punching and ring rolling. Finishing temperature stays above
   1000 C. Reheat rather than finish cold.
4. Solution annealing. 1150 to 1200 C, soak by section, then rapid water quench. Mandatory, because
   as-forged 1.4547 has degraded corrosion performance.
5. Testing. Chemistry and PMI, tensile, hardness, ASTM A262 Practice E, optional G48 Method A,
   ultrasonic examination, dimensional report.
6. Finishing and release. Pickling or machining to drawing, marking, heat and lot traceability,
   EN 10204 3.1 or 3.2 certification, export packing.

### Product forms supplied in 1.4547

- Seamless rolled rings and forged rings, including stepped and profiled rings
- Forged flanges: weld neck, blind, slip-on, long weld neck, orifice, special drawings
- Forged round bars, shafts, spindles, eccentric shafts and crankshafts
- Forged discs, disks, blanks and gear blanks
- Forged sleeves, bushings, hollow bars, forged tubes and forged pipe
- Tube sheets, nozzles, manifolds, headers and heat-exchanger components
- Valve bodies, valve stems, seat rings, balls, plugs and valve blocks

Sizes are quoted against the drawing. Send the dimensions and we will confirm what the press and ring
mill can hold, together with weight and lead time.

## Machining and welding

Machining. 1.4547 runs on the same equipment used for 300-series stainless steel, but it work-hardens
fast. Use rigid set-ups and sharp positive-rake tooling, keep the cut under the hardened layer with a
heavy positive feed, run surface speeds at roughly 60 to 70 percent of those used for 316L, and flood
with coolant. Do not let the tool dwell in the cut.

Welding. 1.4547 welds readily by GTAW, GMAW, SMAW and plasma processes. Molybdenum segregates during
solidification, so matching filler leaves the weld metal under-alloyed and lower in pitting resistance
than the parent material. Use an over-alloyed nickel-base filler instead, normally ERNiCrMo-3
(Alloy 625) or ERNiCrMo-4 (Alloy C-276) to AWS A5.14. Keep heat input low and interpass temperature
below about 150 C. No pre-heat is needed. Post-weld heat treatment is not normally required or wanted,
and a full solution anneal, if applied, must be followed by a rapid quench.

## Where 1.4547 forgings are used

- Offshore and subsea: seawater lift and firewater systems, risers, manifolds, subsea and deepwater
  production hardware, topside piping components.
- Desalination and water: MSF and high-pressure reverse-osmosis plant, seawater piping, demineralised
  water production, waste-water treatment.
- Chemical process: pressure vessels, reactors, heat exchangers and separators handling sulphuric,
  phosphoric, organic and mixed acids with chlorides.
- Power and FGD: flue-gas desulphurisation absorbers, ducting and internals, turbine and gas-compressor
  components, generator hardware.
- Pulp and paper: bleach-plant equipment exposed to chlorine dioxide and chloride-bearing white liquor.
- Valves and rotating parts: ball, gate, globe, check and plug valve bodies, stems and seat rings,
  gearbox and power-transmission components.

## 1.4547 against 316L, 904L, duplex 2205 and Alloy 625

| Alloy | UNS | Mo, % | PREN, typical | Relative cost | Best suited to |
| --- | --- | --- | --- | --- | --- |
| 316L | S31603 | 2.0 to 3.0 | 24 | 1.0x | General service, low chloride |
| Duplex 2205 | S32205 | 3.0 to 3.5 | 35 | 1.2 to 1.6x | Strength-driven, moderate chloride |
| 904L | N08904 | 4.0 to 5.0 | 34 | 2.0 to 2.5x | Sulphuric acid service |
| 1.4547 | S31254 | 6.0 to 7.0 | 43 | 2.5 to 3.5x | Seawater, brine, FGD, mixed acids |
| Super duplex 2507 | S32750 | 3.0 to 5.0 | 42 | 2.5 to 3.5x | Seawater where high strength is needed |
| Alloy 625 | N06625 | 8.0 to 10.0 | 51 | 6 to 9x | Severe or reducing media, high temperature |

Relative cost is indicative of forged-bar pricing and moves with the nickel and molybdenum markets.
Where a 6Mo austenitic and a super duplex both qualify on PREN, 1.4547 is usually preferred for
weldability and toughness, and 2507 where the higher yield strength cuts wall thickness.

## Testing, inspection and certification

- Ultrasonic examination to EN 10228-3, SEP 1921, ASTM A388 or ASME Section V, at the quality class
  stated on the order.
- Chemical analysis, ladle and product, plus positive material identification by XRF or OES on every
  piece where required.
- Mechanical testing: tensile, hardness and, on request, Charpy V-notch impact down to -46 C.
- Corrosion testing: ASTM A262 Practice E for intergranular attack, ASTM G48 Method A at 40 C for
  pitting, to NORSOK M-630 practice.
- Surface and dimensional: liquid penetrant examination to ASTM E165, full dimensional report against
  the drawing.
- Certification: EN 10204 3.1 mill certificate as standard. EN 10204 3.2 with third-party endorsement
  from TUV, BV, DNV, LR, ABS or SGS on request.
- Traceability: heat number, lot number and hard stamping carried from melt to despatch.

## Questions and answers

### What is 1.4547 stainless steel?

1.4547 is a high-molybdenum, nitrogen-alloyed super-austenitic stainless steel, named
X1CrNiMoCuN20-18-7 in EN 10088 and numbered UNS S31254 in ASTM standards. It holds roughly 20 percent
chromium, 18 percent nickel, 6 to 7 percent molybdenum, 0.2 percent nitrogen and 0.5 to 1.0 percent
copper, which gives a PREN of 42 to 44 and strong resistance to pitting, crevice corrosion and chloride
stress corrosion cracking.

### Is 1.4547 the same as 254 SMO and ASTM A182 F44?

They describe the same alloy. 1.4547 is the EN material number, UNS S31254 is the ASTM and UNS number,
F44 is the forging grade designation in ASTM A182, and 254 SMO is Outokumpu's registered trade name.
The EN and ASTM chemical ranges differ slightly: EN allows molybdenum to 7.0 percent and nitrogen to
0.25 percent, while ASTM caps them at 6.5 and 0.22 percent. Dual-certified material is produced to the
narrower of the two.

### What is the PREN value of 1.4547?

Using PREN = %Cr + 3.3 x %Mo + 16 x %N, the minimum specification limits give 42.2 and a typical
production heat gives about 43.3, so published datasheets quote a band of 42 to 44. That puts 1.4547
well above 316L at about 24 and 904L at about 34, and level with super duplex 2507.

### What heat treatment do 1.4547 forgings need?

Solution annealing at 1150 to 1200 C followed by a rapid water quench, with soak time set by section
thickness. This dissolves the intermetallic phases formed during forging and restores full corrosion
resistance. 1.4547 should never be supplied or put into service as-forged, and slow cooling from the
annealing temperature is not acceptable.

### Which filler metal should be used to weld 1.4547?

An over-alloyed nickel-base filler, normally ERNiCrMo-3 (Alloy 625) or ERNiCrMo-4 (Alloy C-276) to
AWS A5.14. Matching filler is avoided because molybdenum segregates during solidification and leaves
the weld metal with lower pitting resistance than the parent material. Keep heat input low and
interpass temperature below about 150 C. No pre-heat and no post-weld heat treatment are required.

### Is 1.4547 magnetic?

No. In the solution annealed condition 1.4547 is fully austenitic and effectively non-magnetic, with a
relative magnetic permeability of about 1.0. Heavy cold work can raise it slightly, but the grade is
stable compared with 304 or 316.

### What is the maximum service temperature of 1.4547?

Pressure design codes list allowable stresses for UNS S31254 up to about 425 C (800 F). Above roughly
500 C, prolonged exposure risks precipitation of sigma and chi intermetallic phases, which embrittles
the material and cuts corrosion resistance. For sustained high-temperature service, pick a
heat-resistant grade or a nickel alloy instead.

### What is the minimum order quantity and lead time for 1.4547 forgings?

Jiangyin Jiangnan Metal Co., Ltd. produces 1.4547 forgings to customer drawings from single prototype
pieces to series production, with no fixed minimum quantity. Lead time depends on billet availability,
section size and the inspection and test plan. Send the drawing or the dimensions to
sales@steelforgepieces.com or call 0086-189-2135-9659 for a confirmed schedule and price.

### Who supplies 1.4547 open-die forgings from China?

Jiangyin Jiangnan Metal Co., Ltd., an open-die forging factory at No. 1 Chengxiqiao Road, Zhouzhuang
Town, Jiangyin City, Jiangsu Province, China, manufactures and exports 1.4547 (UNS S31254,
ASTM A182 F44) forged rings, seamless rolled rings, flanges, bars, discs, shafts, sleeves and tube
sheets worldwide. Phone 0086-189-2135-9659, email sales@steelforgepieces.com, web
www.steelforgepieces.com.

## Supplier

Jiangyin Jiangnan Metal Co., Ltd., open-die forging factory.

- Address: No. 1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
- Telephone, WhatsApp and WeChat: 0086-189-2135-9659
- Email: sales@steelforgepieces.com
- Website: https://www.steelforgepieces.com/
- Business hours: Monday to Saturday, 08:30 to 18:00 China Standard Time (UTC+8)

Send the drawing, or just the grade, dimensions, quantity and the certification you need. Quotations
normally come back within one working day.

## Related grades

- [A182 F44](https://www.steelforgepieces.com/Stainless-Steel/A182-F44.html)
- [904L](https://www.steelforgepieces.com/Stainless-Steel/904L.html)
- [A182 F51 (2205)](https://www.steelforgepieces.com/Stainless-Steel/A182-F51.html)
- [A182 F53 (2507)](https://www.steelforgepieces.com/Stainless-Steel/A182-F53.html)
- [A182 F61](https://www.steelforgepieces.com/Stainless-Steel/A182-F61.html)
- [Sanicro 28](https://www.steelforgepieces.com/Stainless-Steel/Sanicro-28.html)
- [Alloy 24](https://www.steelforgepieces.com/Stainless-Steel/Alloy-24.html)
- [Incoloy 926](https://www.steelforgepieces.com/Nickel-Alloy/Incoloy-926.html)
- [Alloy 31](https://www.steelforgepieces.com/Nickel-Alloy/Alloy-31.html)
- [Inconel 625](https://www.steelforgepieces.com/Nickel-Alloy/Inconel-625.html)
- [Incoloy 825](https://www.steelforgepieces.com/Nickel-Alloy/Incoloy-825.html)
- [A286](https://www.steelforgepieces.com/Stainless-Steel/A286.html)

## Sources and notes

Data compiled from EN 10088, EN 10222-5, ASTM A182, ASTM A240, ASTM A479, NORSOK M-630, and the mill
certificates of material supplied by this factory. Values here are for guidance. The governing purchase
specification and its current edition take precedence.

Cite as: Jiangyin Jiangnan Metal Co., Ltd., "1.4547 Forgings (UNS S31254 / ASTM A182 F44)",
https://www.steelforgepieces.com/Stainless-Steel/1.4547.html