## Summary

Jiangyin Jiangnan Metal Co., Ltd. melts and open-die forges 1.4438 stainless steel in one works in Jiangyin, Jiangsu, China. 1.4438 (EN name X2CrNiMo18-15-4) is a low-carbon, 3–4 % molybdenum austenitic stainless steel with a higher nickel content than 316L, used where chloride pitting and crevice corrosion outrun the 316L family. It is supplied as seamless rolled rings to 6,000 mm outside diameter, forged rings, flanges, shafts, discs, tube sheets, sleeves, bushings, bars and valve parts, in single pieces up to 30 tonnes, with EN 10204 3.1 or 3.2 certification.

## Key facts

| Item | Value |
| --- | --- |
| EN material number | 1.4438 |
| EN designation | X2CrNiMo18-15-4 |
| Nearest UNS number | S31703 (AISI 317L) |
| Nearest ASTM forging grade | ASTM A182 F317L |
| Governing standards | EN 10088-2:2005, EN 10088-3:2014 |
| Type | Low-carbon austenitic stainless steel |
| PREN (Cr + 3.3Mo + 16N) | approx. 27 to 34, typically 31 |
| Maximum rolled ring OD | 6,000 mm |
| Maximum single-piece weight | 30,000 kg |
| Minimum order | 10 kg, no minimum piece count |
| Typical lead time | 20 to 45 days |
| Certification | EN 10204 3.1 standard; 3.2 witnessed on request |
| Class approvals held by the works | CCS, BV, DNV, LR, NK |

## Chemical composition (% by mass)

| Element | EN 10088-3 (bars, forgings) | EN 10088-2 (plate, strip) | ASTM A182 F317L / UNS S31703 |
| --- | --- | --- | --- |
| Carbon, C | ≤ 0.030 | ≤ 0.030 | ≤ 0.030 |
| Silicon, Si | ≤ 1.00 | ≤ 1.00 | ≤ 1.00 |
| Manganese, Mn | ≤ 2.00 | ≤ 2.00 | ≤ 2.00 |
| Phosphorus, P | ≤ 0.045 | ≤ 0.045 | ≤ 0.045 |
| Sulphur, S | ≤ 0.030 | ≤ 0.015 | ≤ 0.030 |
| Chromium, Cr | 17.5 – 19.5 | 17.5 – 19.5 | 18.0 – 20.0 |
| Nickel, Ni | 13.0 – 16.0 | 13.0 – 16.0 | 11.0 – 15.0 |
| Molybdenum, Mo | 3.0 – 4.0 | 3.0 – 4.0 | 3.0 – 4.0 |
| Nitrogen, N | ≤ 0.11 | ≤ 0.11 | not specified |
| Iron, Fe | balance | balance | balance |

No niobium, titanium, vanadium, tungsten, copper, aluminium or boron is specified for this grade.

Melting route at this works: 25 t electric arc furnace, 25 t and 50 t ladle furnaces, 30 t and 60 t vacuum oxygen decarburisation. Maximum heat 60 t. Protective-atmosphere electroslag remelting at 3 t and 6 t is available as a second melt where the specification calls for it.

## Mechanical properties, solution annealed, room temperature

| Property | EN 10088-3, +AT, d ≤ 160 mm | ASTM A182 F317L |
| --- | --- | --- |
| 0.2 % proof strength, Rp0.2 | ≥ 200 MPa | ≥ 170 MPa (25 ksi) |
| Tensile strength, Rm | 500 – 700 MPa | ≥ 485 MPa (70 ksi) |
| Elongation, A | ≥ 40 % (longitudinal) | ≥ 30 % in 50 mm |
| Reduction of area, Z | not specified | ≥ 50 % |
| Impact energy, KV | ≥ 100 J (longitudinal) | by agreement |
| Hardness | not a specification requirement; typically 150 to 190 HB as annealed | not specified |

## Physical properties at 20 °C (typical, for design guidance)

| Property | Typical value |
| --- | --- |
| Density | 7.9 – 8.0 g/cm³ |
| Modulus of elasticity | 200 GPa |
| Thermal conductivity | approx. 14 W/(m·K) |
| Specific heat capacity | approx. 470 J/(kg·K) |
| Thermal expansion, 20–100 °C | approx. 16 × 10⁻⁶ /K |
| Magnetic response | non-magnetic when fully annealed |

## Equivalents

| System | Designation | Relationship |
| --- | --- | --- |
| EN / DIN number | 1.4438 | the grade itself |
| EN / DIN name | X2CrNiMo18-15-4 | the grade itself |
| AISI / ASTM type | 317L | nearest equivalent; nickel band differs |
| UNS | S31703 | nearest equivalent; nickel band differs |
| ASTM forging grade | A182 F317L | the forging specification usually ordered against S31703 |
| ASTM plate | A240 317L | plate counterpart |
| ISO | X2CrNiMo18-15-4 | same designation as EN |
| China GB | 022Cr19Ni13Mo3 / 00Cr19Ni13Mo3 | close equivalent |
| Japan JIS | SUS 317L | close equivalent |

1.4438 and UNS S31703 are the nearest equivalents but they are not identical. 1.4438 requires nickel 13.0–16.0 %; S31703 permits 11.0–15.0 %. For dual-certified material the melt has to sit in the overlap: nickel 13.0–15.0 %, chromium 18.0–19.5 %, molybdenum 3.0–4.0 %, carbon 0.030 % maximum. State dual certification on the enquiry, because it is a melt-shop decision that cannot be made once the heat is poured.

## Comparison with adjacent grades

| Grade | Cr % | Ni % | Mo % | Typical PREN | Usual reason to choose it |
| --- | --- | --- | --- | --- | --- |
| 316L / 1.4404 | 16.5–18.5 | 10.0–13.0 | 2.0–2.5 | 24–26 | general corrosion service, lowest cost of the Mo grades |
| 1.4438 / 317L | 17.5–19.5 | 13.0–16.0 | 3.0–4.0 | approx. 31 | warm chlorides, dilute sulphuric and phosphoric acid, FGD |
| 904L / 1.4539 | 19.0–21.0 | 24.0–26.0 | 4.0–5.0 | 34–36 | stronger acid service, copper for reducing acids |
| 254 SMO / F44 | 19.5–20.5 | 17.5–18.5 | 6.0–6.5 | 42–45 | seawater and high-chloride duty |
| F51 / 2205 duplex | 21.0–23.0 | 4.5–6.5 | 2.5–3.5 | 34–36 | double the yield strength, chloride SCC resistance |

Composition bands are nominal and are shown to place 1.4438 in context rather than to specify the neighbouring grades.

## Forging and heat treatment

1.4438 is forged from about 1,150–1,200 °C and finished above 950 °C, then solution annealed and water quenched. ASTM A182 requires F317L to be solution treated at a minimum of 1,040 °C and liquid-quenched to below 260 °C. Typical practice for 1.4438 is 1,040–1,120 °C followed by a water quench fast enough to carry the section through the 850–550 °C range without precipitating chromium carbides or sigma phase.

On heavy sections the quench rate is the critical variable, because the 3–4 % molybdenum makes 1.4438 more willing than 316L to form sigma phase if the core lingers between 850 °C and 550 °C. Heavy tube sheets and rings are often proof-machined before the quench to reduce the mass being cooled.

1.4438 work-hardens readily during machining, so it takes low surface speeds, a constant positive feed, rigid setups and sharp tooling. It is readily welded by the usual austenitic processes; with carbon at 0.030 % maximum a post-weld solution anneal is generally not required for corrosion reasons.

## Product forms and size envelope

| Product form | Size limit | Set by |
| --- | --- | --- |
| Seamless rolled rings | OD 50 mm to 6,000 mm | 6 m radial-axial ring mill |
| Forged rings | sections outside the ring-mill envelope | 6,300 t press, upset and punch |
| Forged flanges | ASME B16.5, B16.47 Series A/B, API 6A | press and ring mill |
| Forged shafts and spindles | up to 14,000 mm turned length | C61160 lathe; 15 m well furnace |
| Discs, tube sheets, covers | up to Ø5,000 mm machined | Ø5,000 mm vertical turning lathe |
| Bars, blocks, billets | round, flat and square | 6,300 / 4,000 / 2,000 t presses |
| Cylinders, sleeves, bushings | bored to Ø1,600 × 10,000 mm | CNC deep-hole drilling machine |
| Valve and wellhead parts | bodies, bonnets, stems, seat rings | press and machine shop |
| Single-piece weight | up to 30,000 kg | 60 t heat size; 6,300 t press |

## Applications

Chemical and petrochemical plant, flue-gas desulphurisation, pulp and paper, oil and gas including offshore and NACE MR0175 / ISO 15156 service, power generation heat exchangers and condensers, pharmaceutical and food processing equipment.

## Testing and certification

Carried out in the on-site laboratory: optical emission spectrometry (ASTM E415), infrared carbon and sulphur analysis (ASTM E1019), positive material identification, tensile testing on 600 kN and 300 kN machines (ASTM A370, ISO 6892), Charpy V-notch impact to −60 °C, ultrasonic testing (ASTM A388, EN 10228-3), magnetic particle (ASTM E709), metallography and grain size (ASTM E112).

Placed with an accredited third-party laboratory: intergranular corrosion (ASTM A262 Practice E or B), pitting resistance (ASTM G48 Method A), intergranular attack (ASTM G28 Method A), bench Brinell or Rockwell hardness, impact testing below −60 °C.

Certification: EN 10204 3.1 as standard; EN 10204 3.2 witnessed by BV, DNV, LR, SGS, TÜV or the customer's own inspector on request. Because the steel is melted on site, the certificate traces the part from its melt number through forging, heat treatment and machining to shipment.

## How to request a quotation

Email sales@steelforgepieces.com with:

1. Grade and governing specification, for example 1.4438 to EN 10088-3, dual certified to ASTM A182 F317L
2. Dimensions, or a drawing (PDF, DWG, DXF, STEP)
3. Quantity and expected repeat volume
4. Delivery condition: as-forged, proof-machined for UT, or finish-machined
5. Heat treatment and testing requirements
6. Certification and destination port

Quotations normally return within two working days.

## Company record

- Legal name: Jiangyin Jiangnan Metal Co., Ltd.
- Business: integrated melting works, open-die forge and ring rolling mill
- Established: 1997
- Employees: 460, including 9 senior engineers, 32 intermediate engineers and 140 technicians
- Plant: No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
- Coordinates: 31.8330, 120.3510
- Melting: EF, LF, VOD, VIM, VAR, ESR; 60 t maximum heat
- Forging: 6,300 t press, 6 m radial-axial ring mill, 30 t maximum piece
- Approvals: CCS, BV, DNV, LR, NK
- Telephone, WhatsApp and WeChat: +86 189 2135 9659
- Email: sales@steelforgepieces.com
- Hours: Monday to Saturday, 08:00 to 17:30 China Standard Time (UTC+8)
- Exports to: North America, Europe, the Middle East, Asia-Pacific

## Standards referenced

- EN 10088-2:2005, Stainless steels, Part 2: Technical delivery conditions for sheet/plate and strip, grade X2CrNiMo18-15-4 (1.4438)
- EN 10088-3:2014, Stainless steels, Part 3: Technical delivery conditions for semi-finished products, bars, rods, wire, sections and bright products, grade X2CrNiMo18-15-4 (1.4438)
- ASTM A182/A182M, Standard Specification for Forged or Rolled Alloy and Stainless Steel Pipe Flanges, Forged Fittings, and Valves and Parts for High-Temperature Service, Grade F317L (UNS S31703)
- ASTM A370 and ISO 6892 for mechanical testing; ASTM A388 and EN 10228-3 for ultrasonic examination; ASTM A262, G28 and G48 for corrosion testing; EN 10204 for certification

Composition and mechanical values are the limits set by the cited standards. Physical properties are typical values for design guidance and are not certified acceptance criteria. Equivalence between national standards is never exact, so the purchase order must state which specification governs.