# 20Mn6 (1.1169) Steel Forgings

**Supplier:** Jiangyin Jiangnan Metal Co., Ltd., open-die forging factory
**Address:** No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
**Telephone:** +86 189 2135 9659
**Email:** sales@steelforgepieces.com
**Page:** https://www.steelforgepieces.com/Alloy-Steel/20Mn6.html
**Last reviewed:** 2026-09-10

---

20Mn6 (material number 1.1169) is a manganese-alloyed special steel to DIN 17200, with a nominal
analysis of 0.17-0.23 % carbon and 1.30-1.60 % manganese. It is specified for high-pressure vessels
and pressure-bearing tube in service down to -100 degrees Celsius, where toughness at low temperature
counts for more than hardness. Jiangyin Jiangnan Metal Co., Ltd. forges 20Mn6 to customer drawing as
bars, hollow bars, seamless rolled rings, discs, blocks, shafts and flanges.

## 20Mn6 at a glance

- **Designation:** 20Mn6 is the DIN designation. The matching Werkstoff (material) number is 1.1169.
- **Chemistry:** 0.17-0.23 % C, 0.30-0.60 % Si, 1.30-1.60 % Mn, P and S each 0.035 % maximum, balance Fe.
- **Classification:** non-alloy special steel. Manganese is the only significant addition, so there is no chromium, nickel or molybdenum in the analysis.
- **Heat treatment:** normalise 880-910 C air cooled, or harden in water at 860-890 C and temper at 500-650 C.
- **Typical use:** high-pressure vessels and tube rated for service down to -100 C.
- **Minimum order:** one piece, forged to drawing.
- **Certificate:** EN 10204 3.1 as standard, 3.2 with third-party inspection on request.

## What is 20Mn6 steel?

20Mn6 is a low-carbon steel that gets its properties from manganese rather than from a conventional
alloy package. At 1.30-1.60 % Mn it carries roughly three times the manganese of a plain C22 carbon
steel. That raises hardenability and tensile strength while the carbon stays low enough for the steel
to weld and machine without trouble. DIN files it as a non-alloy special steel: the word "special"
refers to the tight limits on phosphorus and sulphur, not to any alloy content.

Pressure equipment is where the grade earns its place. A designer gets a workable strength level and
dependable low-temperature toughness without paying for a chromium-molybdenum steel, and the fabricator
gets something that behaves predictably under the torch. The limitation is section size. With no
molybdenum to slow the transformation, through-hardening drops away quickly as the forging gets
heavier, so thick 20Mn6 sections are normally supplied normalised rather than fully quenched and
tempered.

## 20Mn6 chemical composition

Ladle analysis in weight percent, to DIN 17200. Balance iron.

| Element | Symbol | Min % | Max % | Role in this grade |
|---|---|---|---|---|
| Carbon | C | 0.17 | 0.23 | Kept low for weldability and low-temperature toughness |
| Silicon | Si | 0.30 | 0.60 | Deoxidiser, plus a little solid-solution strength |
| Manganese | Mn | 1.30 | 1.60 | Principal alloying element for hardenability and strength |
| Phosphorus | P | - | 0.035 | Residual, held down to protect toughness |
| Sulphur | S | - | 0.035 | Residual, held down to protect transverse ductility |

Product analysis taken on a finished forging may deviate within the tolerances of the applicable
standard. Each heat is supplied with its own certificate of analysis.

## 20Mn6 mechanical properties

Indicative room-temperature properties, longitudinal test piece. Values depend on ruling section and
delivery condition. The EN 10204 certificate issued with the forging is the governing document.

| Condition | Ruling section | Rp0.2 min. | Rm | A5 min. | KV at -40 C | Hardness |
|---|---|---|---|---|---|---|
| Normalised | up to 100 mm | 295 MPa | 490-630 MPa | 22 % | 27 J | 140-190 HB |
| Normalised | 100-250 mm | 275 MPa | 470-610 MPa | 21 % | 27 J | 135-185 HB |
| Normalised | 250-400 mm | 255 MPa | 450-590 MPa | 20 % | 27 J | 130-180 HB |
| Quenched and tempered | up to 100 mm | 390 MPa | 590-740 MPa | 20 % | 40 J | 175-220 HB |
| Quenched and tempered | 100-250 mm | 345 MPa | 550-700 MPa | 19 % | 35 J | 165-210 HB |

Impact testing at other temperatures, down to -100 C, is carried out on request. Transverse testing,
through-thickness testing and quarter-radius sampling can all be specified on the order.

## 20Mn6 heat treatment

| Operation | Temperature | Cooling | Purpose |
|---|---|---|---|
| Normalising | 880-910 C | Still air | Refine grain after forging. Usual condition for heavy sections |
| Hardening | 860-890 C | Water quench | Transform to martensite and bainite |
| Tempering | 500-650 C | Air | Set final strength and restore toughness |
| Soft annealing | 650-700 C | Furnace cool | Lower hardness ahead of heavy machining |
| Stress relief | 550-650 C | Furnace cool to 400 C, then air | Relieve machining and welding stresses |

Water quenching is hard on abrupt section changes. Where a drawing has thin webs next to heavy hubs,
or sharp internal corners, we look at the geometry before committing to a hardening route and will
often recommend normalised or normalised-and-tempered delivery instead.

## Forging 20Mn6

| Parameter | Value |
|---|---|
| Start forging temperature | 1150-1200 C |
| Finish forging temperature | not below 850 C |
| Minimum forging ratio | 3:1, higher on request |
| Post-forge cooling | Still air, or slow cool in an insulated pit for heavy sections |
| Post-forge condition | Normalised as standard, unless the order calls for something else |

Ring geometries are pierced and expanded on a radial-axial mill, which puts the grain flow around the
circumference instead of cutting across it.

## What is 20Mn6 equivalent to?

There is no exact one-to-one international equivalent. The grades below are the closest
carbon-manganese steels by chemical analysis. This is an indicative comparison, not a certified
substitution.

| Standard | Grade | Carbon % | Manganese % | How close |
|---|---|---|---|---|
| DIN 17200 (Germany) | 20Mn6 | 0.17-0.23 | 1.30-1.60 | The grade itself |
| Werkstoff-Nr. | 1.1169 | 0.17-0.23 | 1.30-1.60 | Same steel, material-number form |
| AISI / SAE (USA) | 1524 | 0.19-0.25 | 1.35-1.65 | Nearest US carbon-manganese grade |
| AISI / SAE (USA) | 1522 | 0.18-0.24 | 1.10-1.40 | Leaner in manganese |
| GB/T 3077 (China) | 20Mn2 | 0.17-0.24 | 1.40-1.80 | Nearest Chinese grade, richer in manganese |
| DIN (Germany) | 20Mn5 / 1.1133 | 0.17-0.23 | 1.10-1.40 | Leaner neighbour in the same family |

Mechanical acceptance, impact requirements, permitted residuals and pressure-equipment approval all
differ between standards. Confirm any substitution with your design authority before ordering.

### 20Mn6 vs 20Mn5

Both sit in the same low-carbon manganese family, and the number after "Mn" is roughly the manganese
content multiplied by four. 20Mn6 carries the higher manganese of the two, which buys more
hardenability and a higher strength level in the same section at some cost in weldability. Where a
drawing calls for 20Mn5 and only 20Mn6 is available, the substitution usually runs toward higher
strength, but the weld procedure and the impact requirement both need checking first.

## 20Mn6 forged products

Forged to drawing or specification. Not held as catalogue stock. Minimum order one piece.

| Product form | Also called | Size range | Single-piece weight |
|---|---|---|---|
| Forged bar | Round, square, flat, rectangular, hex bar | 80-1200 mm dia. or across flats, up to 8000 mm long | 20-20,000 kg |
| Hollow forgings | Hollow bar, sleeve, bush, bushing, cylinder, barrel, casing, shell, hub, housing | 150-2500 mm OD, 50-2000 mm ID | up to 20,000 kg |
| Seamless rolled rings | Radial-axial rolled rings | 200-3000 mm OD, height up to 1000 mm | up to 15,000 kg |
| Forged rings | Mandrel-forged and punched rings | 200-3000 mm OD | up to 20,000 kg |
| Discs, blocks and plates | Forged disc, disk, block, slab | 200-2500 mm dia., or to drawing | up to 20,000 kg |
| Shafts | Gear shaft, pinion shaft, spindle, stepped shaft | up to 8000 mm long | up to 20,000 kg |
| Forged flanges | Weld-neck, slip-on, blind, custom profile | 100-3000 mm OD | up to 10,000 kg |

## How a 20Mn6 forging is made

1. **Drawing review and quotation.** Forgeability, ruling section, machining allowance and heat-treatment route are checked before pricing.
2. **Steel making and material certification.** Melt sourced to the required analysis, certificate traceable to heat number.
3. **Heating and open-die forging.** Billet soaked to 1150-1200 C, then upset and drawn under open dies.
4. **Ring rolling.** For ring geometries, the pierced blank is rolled radially and axially to final proportions.
5. **Heat treatment.** Normalising, or hardening and tempering, to whichever condition the specification calls for.
6. **Testing and inspection.** Chemical analysis, mechanical testing, hardness, dimensional check, plus ultrasonic or magnetic-particle examination where specified.
7. **Machining.** Rough or finish machining to drawing.
8. **Documentation and despatch.** Certificates issued against the heat, parts marked, packed and shipped.

## Where 20Mn6 is used

- High-pressure vessel shells, heads and nozzle forgings
- Pressure-bearing tube and pipe components for cold and cryogenic service
- Flanges and closures on vessels rated below ambient temperature
- Machine components needing a weldable medium-strength steel in forged form
- Gear and pinion shafts, spindles and hubs in general engineering

Suitability for a particular pressure code, whether PED, ASME or GB 150, depends on the approvals held
for the grade and for the manufacturer, not on the analysis alone.

## Questions

**What is the material number for 20Mn6?**
1.1169. Same steel, two names: 20Mn6 is the DIN designation, 1.1169 is the Werkstoff number printed on
the mill certificate.

**Is 20Mn6 an alloy steel or a carbon steel?**
DIN classifies it as a non-alloy special steel. Manganese is the only significant addition, so it
behaves as an enhanced carbon-manganese steel rather than a true alloy steel.

**Can 20Mn6 be welded?**
Yes, with normal procedures. Carbon sits at 0.17-0.23 %, which is comfortable territory, but the
manganese pushes the carbon equivalent up far enough that heavier sections want preheat and a
controlled interpass temperature. Work out CEV from the actual heat analysis rather than from the middle
of the specification range, because a heat running at 1.58 % Mn behaves differently from one at 1.32 %.
On pressure parts post-weld heat treatment is normally called for anyway.

**What is the minimum order quantity?**
One piece. Open dies and a ring mill both work from a single billet. Repeat bar sizes get cheaper above
roughly 500 kg.

**Do you supply EN 10204 3.1 or 3.2 certificates?**
3.1 as standard with every order. For 3.2 we arrange third-party inspection through SGS, BV, TUV or
Lloyd's Register. Flag it at enquiry stage so the witness points go into the schedule.

**How long does a 20Mn6 forging take?**
Rough-forged and normalised parts usually run 25 to 35 days from order. Parts needing quenching and
tempering, machining to drawing, or third-party witnessed testing typically run 35 to 45 days.

**Do you hold 20Mn6 in stock?**
No. Everything is forged to order, so size, forging ratio and heat-treatment condition follow your
drawing rather than the rack.

**What information is needed to quote?**
A drawing or dimensioned sketch, the quantity, the delivery condition, the machining allowance if the
part is rough-forged, the certificate type, and the standard or pressure code the part is built to.

## Other grades

- [42CrMo4 (1.7225)](https://www.steelforgepieces.com/Alloy-Steel/42CrMo4.html) - chromium-molybdenum step up when 20Mn6 cannot reach the strength or section size required
- [AISI 4140](https://www.steelforgepieces.com/Alloy-Steel/AISI-4140.html) - American counterpart to 42CrMo4
- [AISI 4130](https://www.steelforgepieces.com/Alloy-Steel/AISI-4130.html) - leaner chromium-molybdenum grade, better weldability
- [34CrMo4 (1.7220)](https://www.steelforgepieces.com/Alloy-Steel/34CrMo4.html) - European equivalent of 4130
- [AISI 8630](https://www.steelforgepieces.com/Alloy-Steel/AISI-8630.html) - wellhead and subsea components
- [34CrNiMo6 (1.6582)](https://www.steelforgepieces.com/Alloy-Steel/34CrNiMo6.html) - deep hardening through heavy section
- [18CrNiMo7-6](https://www.steelforgepieces.com/Alloy-Steel/18CrNiMo7-6.html) - case-hardening gear steel
- [All alloy steel grades](https://www.steelforgepieces.com/Alloy-Steel/)

## Contact

Jiangyin Jiangnan Metal Co., Ltd.
No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
Telephone, WhatsApp and WeChat: +86 189 2135 9659
Email: sales@steelforgepieces.com
Web: https://www.steelforgepieces.com/

---

Technical data on this page is compiled from published standards for 20Mn6 / 1.1169 and is given for
guidance. It is not a warranty of properties. The certificate issued with each forging governs.