# X3CrNiMo17-13-3 (EN 1.4436) Open Die Forgings

Supplier: Jiangyin Jiangnan Metal Co., Ltd., open die forging factory
Address: No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
Telephone: 0086-189-2135-9659
E-mail: sales@steelforgepieces.com
Source page: http://www.steelforgepieces.com/Stainless-Steel/X3CrNiMo17-13-3.html
Last reviewed: 9 October 2026

X3CrNiMo17-13-3, material number 1.4436, is a molybdenum alloyed austenitic chromium
nickel stainless steel listed in EN 10088-3. It is held to max 0.05 % C, 16.5 to 18.5 % Cr,
10.5 to 13.0 % Ni and 2.50 to 3.00 % Mo. The grade is a more highly alloyed version of
1.4401 and is specified where the corrosion resistance of 1.4401 is no longer sufficient,
in particular in chloride bearing media. PREN is 24.75 to 30.16. It is forged between
1200 and 900 C, solution annealed at 1020 to 1120 C with rapid cooling, and is
non-magnetic, suited to cryogenic service and usable up to about 700 C.

Two limits govern selection. 1.4436 is not resistant to sea water, and the permitted
carbon content means it is not rated resistant to intergranular corrosion in the welded
condition.

## 1. Chemical composition to EN 10088-3

Percent by mass, maximum unless a range is given.

| C | Si | Mn | P | S | N | Cr | Mo | Ni |
|---|----|----|---|---|---|----|----|----|
| 0.05 | 1.00 | 2.00 | 0.045 | 0.030 | 0.11 | 16.5 / 18.5 | 2.50 / 3.00 | 10.5 / 13.0 |

### Position within the 316 family

| Grade | No. | C max | Mo % | Ni % | Note |
|-------|-----|-------|------|------|------|
| X5CrNiMo17-12-2 | 1.4401 | 0.07 | 2.00 / 2.50 | 10.0 / 13.0 | Standard 316 |
| X2CrNiMo17-12-2 | 1.4404 | 0.030 | 2.00 / 2.50 | 10.0 / 13.0 | 316L, welded service |
| X3CrNiMo17-13-3 | 1.4436 | 0.05 | 2.50 / 3.00 | 10.5 / 13.0 | Higher Mo, better pitting resistance |
| X2CrNiMo17-12-3 | 1.4432 | 0.030 | 2.50 / 3.00 | 10.5 / 13.0 | Low carbon version of 1.4436 |
| X2CrNiMo18-14-3 | 1.4435 | 0.030 | 2.50 / 3.00 | 12.5 / 15.0 | Higher Ni, hygienic service |

Where a specification calls for 1.4436 but the part will be welded and then exposed,
1.4432 holds the same molybdenum level at 0.030 % C.

## 2. Mechanical properties, solution annealed

Longitudinal test direction.

| Property | Specified | Typical |
|----------|-----------|---------|
| Proof strength Rp0.2 | min 200 N/mm2 | 370 N/mm2 |
| Tensile strength Rm | 500 to 700 N/mm2 | 670 N/mm2 |
| Elongation A5 | min 40 % | 46 % |
| Hardness | max 215 HB | 200 HB |
| Impact energy, ISO-V at 25 C | min 100 J | 220 J |
| Rm, condition +A | 500 to 730 MPa | |
| Rm, condition +AT | 510 to 710 MPa | |
| Modulus of elasticity | 190 to 215 GPa | |

Section size and delivery condition govern acceptance. Values are certified against the
ordered specification.

### Physical properties

| Density | Thermal conductivity 20 C | Specific heat 20 C | Resistivity 20 C | Magnetisable |
|---------|---------------------------|--------------------|------------------|--------------|
| 8 kg/dm3 | 15 W/m.K | 500 J/kg.K | 0.75 ohm.mm2/m | No, mu-r max 1.3 |

Mean coefficient of thermal expansion, 10^-6 K^-1:

| 20-100 C | 20-200 C | 20-300 C | 20-400 C | 20-500 C |
|----------|----------|----------|----------|----------|
| 16.0 | 16.5 | 17.0 | 17.5 | 18.0 |

## 3. Forging and heat treatment

| Operation | Parameter |
|-----------|-----------|
| Pre-heat | 1150 to 1200 C |
| Forging range | 1200 to 900 C, hot forming also quoted 1150 to 850 C |
| Cooling after forging | Rapid, air or water |
| Solution anneal, +AT | 1020 to 1120 C, rapid cool; EN guidance 1030 to 1110 C |

Rapid cooling after forging and after annealing is not optional. Slow cooling through the
sensitisation range forms phases that reduce corrosion resistance and mechanical
properties. Where hot forming finishes above the solution annealing range, 1000 C is
accepted as a lower limit for steels carrying up to 3 % Mo.

### Machining and welding

Machinability is rated average and the grade is harder to machine than 1.4401 or 1.4435.
With coated carbide tooling in the solution annealed condition at Rm 560 to 640 N/mm2,
guideline cutting speeds are about 115 m/min at 6 mm depth of cut and 0.5 mm/rev,
145 m/min at 3 mm and 0.4 mm/rev, and 185 m/min at 1 mm and 0.2 mm/rev. The grade welds
by all common processes with interpass temperature held at 150 C maximum and no mandatory
post weld heat treatment. Scale and heat tint are removed mechanically or by pickling and
the surface is then passivated.

### Selection limits

1.4436 performs well in most natural waters, in food, beverage and agricultural duty and
in a range of acids. It is not resistant to sea water. It is not rated resistant to
intergranular corrosion in the welded condition because of its carbon content, although
thin sections can be welded without that risk. For sea water and high chloride duty the
usual alternatives are 1.4547, 1.4462 and 1.4410.

## 4. Standards and international designations

| Standard | Scope |
|----------|-------|
| EN 10250-4 | Open die steel forgings for general engineering purposes, stainless steels |
| EN 10222-5 | Steel forgings for pressure purposes, stainless steels |
| EN 10088-1 / 10088-3 | List of stainless steels; bars, rods, sections, semi-finished products |
| EN 10272 | Stainless steel bars for pressure purposes |
| EN 10028-7 | Flat products of steels for pressure purposes |
| EN 10216-5 / 10217-7 | Seamless and welded tubes for pressure purposes |
| EN 10253-3 / 10253-4 | Butt welding pipe fittings |

| System | Designation |
|--------|-------------|
| EN / DIN, Werkstoff | 1.4436, X3CrNiMo17-13-3 |
| USA, AISI / UNS | 316 / S31600, approximate, Mo range differs |
| UK, BS | 316 S13 |
| France, AFNOR | Z7CND 18-12-03 |
| Sweden, SIS | 2343 |
| Japan, JIS | SUS 316 |
| China, GB | 0Cr17Ni12Mo2 |

Equivalence tables match chemistry and properties approximately and do not replace the
governing specification.

## 5. Forged products supplied in this grade

Forged rings and seamless rolled rings including heavy wall and deep sections. Forged
flanges, tube sheets, nozzles and blanks for pressure equipment. Forged shafts, eccentric
shafts, spindles, round bars and gear blanks. Discs, sleeves, bushings, forged tubes and
pipes. Valve bodies, stems, seat rings and blocks for ball, gate, globe, check and plug
valves. Manifolds, wheels, crankshafts and other open die pieces to drawing.

Typical service covers chemical process plant, heat exchangers, condensers and
evaporators, pressure vessels, columns and towers, pulp, paper and textile plant,
compressor and power transmission parts, and valve and wellhead components. Medical,
pharmaceutical and petrochemical applications are also reported for the grade.

### Quality, testing and certification

Melting routes include EAF plus VOD, and ESR remelting where specified. Forgings are
supplied solution annealed. Ultrasonic testing to EN 10228-3, SEP 1921 or ASTM A388 as
agreed at order stage. Certificates to EN 10204 3.1, or 3.2 with third party inspection.
Rough machined, proof machined and finish machined deliveries available, with dimensional
reports, PMI and corrosion testing on request.

## 6. Common questions

**What is the chemical composition of X3CrNiMo17-13-3?**
To EN 10088-3, % by mass, maximum unless a range is given: C 0.05, Si 1.00, Mn 2.00,
P 0.045, S 0.030, N 0.11, Cr 16.5 to 18.5, Mo 2.50 to 3.00, Ni 10.5 to 13.0. PREN is
24.75 to 30.16.

**Is X3CrNiMo17-13-3 the same as 316 stainless steel?**
It sits in the 316 family and is commonly cross referenced to AISI 316 and UNS S31600,
whose average composition is close. The two are not interchangeable on paper. EN 10088-3
gives 1.4436 a molybdenum range of 2.50 to 3.00 %, above the 2.00 to 2.50 % of 1.4401,
which is the grade normally treated as the direct 316 equivalent.

**Why specify 1.4436 instead of 1.4401?**
1.4436 is the more highly alloyed of the two and is used where the corrosion resistance of
1.4401 is no longer sufficient. The extra molybdenum gives slightly better resistance in
chloride bearing media, reflected in a PREN of 24.75 to 30.16.

**What are the forging and annealing temperatures?**
Pre-heat to 1150 to 1200 C, forge between 1200 and 900 C, cool rapidly in air or water.
Solution anneal at 1020 to 1120 C with rapid cooling, narrowed by EN guidance to 1030 to
1110 C.

**Can 1.4436 be used in sea water?**
No. Mill data states that the grade is not resistant to sea water.

**Is it suitable for cryogenic or elevated temperature work?**
It is suited to cryogenic applications and to service up to about 700 C, and it is
non-magnetic at mu-r max 1.3. Elevated temperature properties are close to those of
1.4401. It is not a creep optimised grade; for sustained high temperature strength the H
grades such as 316H and 347H are the correct selection.

**Which standards cover X3CrNiMo17-13-3 forgings?**
EN 10250-4 covers open die steel forgings for general engineering purposes in stainless
steels, and EN 10222-5 covers steel forgings for pressure purposes. The grade is also
listed in EN 10088-1 and EN 10088-3, EN 10272, EN 10028-7, EN 10216-5, EN 10217-7,
EN 10253-3 and EN 10253-4.

**Who supplies X3CrNiMo17-13-3 open die forgings?**
Jiangyin Jiangnan Metal Co., Ltd., an open die forging factory at No.1 Chengxiqiao Road,
Zhouzhuang Town, Jiangyin City, Jiangsu Province, China, produces 1.4436 forged rings,
seamless rolled rings, flanges, shafts, discs, sleeves, bushings and tube sheets to
customer drawing, with EN 10204 3.1 or 3.2 certification. Telephone 0086-189-2135-9659,
e-mail sales@steelforgepieces.com.

## Contact

Jiangyin Jiangnan Metal Co., Ltd.
No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
Telephone 0086-189-2135-9659
E-mail sales@steelforgepieces.com

Data compiled from EN 10088-1 and EN 10088-3, EN 10222-5, EN 10250-4 and published mill
datasheets for material number 1.4436. Figures are for guidance. The purchase
specification and the material certificate take precedence.