# X2CrNiMoN18-12-4 Forgings (EN 1.4434 / UNS S31753 / 317LN)

**Supplier:** Jiangyin Jiangnan Metal Co., Ltd., open-die forging factory
**Address:** No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
**Phone:** +86 189-2135-9659
**Email:** sales@steelforgepieces.com
**Canonical page:** http://www.steelforgepieces.com/Stainless-Steel/X2CrNiMoN18-12-4.html
**Last reviewed:** 9 October 2026

X2CrNiMoN18-12-4 (material number 1.4434) is a low-carbon, nitrogen-alloyed austenitic
stainless steel standardised in EN 10088-1, EN 10088-2 and EN 10028-7. Its 3.0 to 4.0
percent molybdenum and 0.10 to 0.20 percent nitrogen give better pitting and crevice
resistance than 316L and a higher proof strength than 317L, while the 0.030 percent
carbon ceiling keeps it resistant to sensitisation after welding. The grade is
equivalent to AISI 317LN and UNS S31753. Jiangyin Jiangnan Metal Co., Ltd. supplies it
as custom forgings with EN 10204 3.1 or 3.2 certification.

Quick reference: Material No. 1.4434 | UNS S31753 | AISI 317LN | JIS SUS 317LN |
KS STS 317LN | GB 022Cr19Ni13Mo4N | ISO 15510 4434-317-53-I | PREN about 32

## 1. Forgings produced in this grade

All parts are made to the customer drawing or dimension list. There is no fixed catalogue.

| Category | Forged items | Typical destination |
|---|---|---|
| Rings | Seamless rolled rings, forged rings, retaining rings, valve seat rings | Pressure vessels, columns, towers, flanged joints |
| Flanges and closures | Forged flanges, blind flanges, nozzles, tube sheets, manifolds | Shell and tube heat exchangers, air receivers, reactors |
| Round sections | Round bars, blocks, billets, forged pipes and tubes, sleeves, bushings | Machining stock, pump and valve bodies |
| Rotating parts | Shafts, eccentric shafts, spindles, crankshafts, gears, rolls | Agitators, gearboxes, compressors, power transmission |
| Flat sections | Discs, disks, wheels, hubs, plates | Valve internals, closure heads, process modules |

## 2. Chemical composition (EN 10088-2 cast analysis, percent by mass)

Single values are maxima. EN 10028-7 specifies the same ranges.

| Element | Min | Max | Function |
|---|---|---|---|
| Carbon (C) | - | 0.030 | Resists sensitisation and intergranular attack after welding |
| Silicon (Si) | - | 1.00 | Deoxidiser |
| Manganese (Mn) | - | 2.00 | Austenite stabiliser, raises nitrogen solubility |
| Phosphorus (P) | - | 0.045 | Residual, restricted |
| Sulphur (S) | - | 0.015 | Residual, restricted for hot workability |
| Chromium (Cr) | 16.5 | 19.5 | Forms the passive film |
| Nickel (Ni) | 10.5 | 14.0 | Austenite stability, acid and stress corrosion resistance |
| Molybdenum (Mo) | 3.0 | 4.0 | Chloride pitting and crevice resistance |
| Nitrogen (N) | 0.10 | 0.20 | Raises proof strength, reinforces pitting resistance |
| Iron (Fe) | Balance | | |

**Ordering note.** Several datasheets circulate a typical analysis of 18.2 Cr, 14 Ni,
4.2 Mo for 317LN. A molybdenum level of 4.2 percent sits outside the EN 10088-2 limit
of 4.0 percent maximum for 1.4434. Qualify the heat against the range above, not
against a nominal figure. A narrower internal window, for example Mo 3.5 percent
minimum to lift PREN, can be set on request.

**PREN.** Calculated PREN is about 32, between standard 316L and the 6 percent
molybdenum superaustenitics. PREN is a comparative index and does not replace
corrosion testing in the actual service chemistry. Real performance depends on
temperature, chloride level, pH and surface finish.

## 3. Mechanical properties

EN 10028-7 minimum values, solution annealed (+AT):

| Product form | Rm (MPa) | Rp0.2 min (MPa) | Rp1.0 min (MPa) | A min (%) |
|---|---|---|---|---|
| Hot rolled plate, t up to 75 mm | 540 to 740 | 270 | 310 | 40 |
| Hot rolled strip, t up to 12 mm | 570 to 770 | 270 | 310 | 35 |
| Cold rolled strip, t up to 6 mm | 570 to 770 | 290 | 320 | 35 |

Charpy V-notch to the same standard: 100 J minimum longitudinal and 60 J minimum
transverse at 20 degrees C, and 60 J minimum transverse at minus 196 degrees C. This
is why the grade is accepted for cryogenic structures as well as ambient process
equipment.

Typical values for the grade, solution annealed: tensile about 660 MPa, Rp0.2 about
310 MPa, elongation about 41 percent, Charpy about 90 J, hardness about 200 HB,
fatigue strength about 270 MPa. These describe the grade and are not guaranteed minima.

Physical properties: density 7.9 to 8.0 g/cm3, modulus of elasticity 200 GPa, shear
modulus about 79 GPa, Poisson ratio about 0.28, thermal conductivity about 15 W/m.K,
specific heat about 470 J/kg.K, thermal expansion about 16 micrometre/m.K, melting
range about 1400 to 1450 degrees C, non-magnetic when annealed.

For forgings, acceptance values are agreed at order stage against the governing
standard, commonly EN 10250-4 for open-die stainless forgings or EN 10272 for bars
for pressure purposes.

## 4. Equivalents and standards

| Region or body | Designation |
|---|---|
| EN steel name | X2CrNiMoN18-12-4 |
| EN material number | 1.4434 |
| USA, AISI and ASTM | 317LN, ASTM A240 Type 317LN |
| USA, UNS | S31753 |
| Japan, JIS | SUS 317LN |
| South Korea, KS | STS 317LN |
| China, GB | 022Cr19Ni13Mo4N |
| ISO 15510 | 4434-317-53-I |

Standards listing 1.4434:

| Standard | Scope |
|---|---|
| EN 10088-1 | List of stainless steels |
| EN 10088-2 | Sheet, plate and strip for general purposes |
| EN 10088-3 | Semi-finished products, bars, rods and sections |
| EN 10028-7 | Flat products for pressure purposes, stainless steels |
| EN 10272 | Stainless steel bars for pressure purposes |
| EN 10250-4 | Open-die steel forgings for general engineering, stainless steels |
| ISO 9328-7, ISO 15510 | International equivalents |
| AD 2000-Merkblatt W 2 | German pressure equipment material approval |

**1.4434 is not 1.4439.** X2CrNiMoN17-13-5 (1.4439) is a separate, higher molybdenum
grade corresponding to 317LMN and UNS S31726. If the specification calls for 317LMN,
the correct grade is 1.4439.

## 5. Manufacturing

**Melting route.** EAF with VOD refining, with ESR remelting available where improved
cleanliness, tighter segregation control or better transverse properties in heavy
sections are required. The route is fixed at order confirmation and stated on the
mill certificate.

**Hot working.** Open-die forging in the austenitic hot working range, with reheating
as needed. Nitrogen-alloyed austenitics work-harden quickly, so reductions and
finishing temperature are planned to leave a structure that fully recrystallises
during solution annealing.

**Solution annealing.** The grade cannot be hardened by heat treatment. Published
practice for 317LN places solution treatment between 1080 and 1175 degrees C followed
by rapid water quenching to hold carbides and intermetallics in solution. Where final
forming finishes below roughly 950 degrees C, a re-solution anneal is needed to
restore corrosion performance. The exact cycle is set per part geometry and section
thickness.

**Machining and welding.** Rigid setups, positive rake, heavy feeds, sharp tooling and
plenty of coolant. Dwelling or rubbing glazes the surface. Welding follows normal
low-carbon austenitic practice, and the 0.030 percent carbon limit means post-weld
annealing is not usually required to avoid sensitisation in thin sections.

**Inspection.** Ultrasonic examination to EN 10228-4, which covers austenitic and
austenitic-ferritic stainless steel forgings. ASTM A388 or SEP 1921 on request.
EN 10228-3 covers ferritic or martensitic forgings and is not the correct reference
for this grade. Certification to EN 10204 3.1, or 3.2 with third party endorsement
such as TUV, BV, LR, DNV or SGS.

## 6. Applications

| Sector | Typical forged components | Reason for the grade |
|---|---|---|
| Chemical and petrochemical | Rolled rings, shafts, nozzles, reactor internals | Resistance to organic, sulphuric and phosphoric acids |
| Pressure equipment | Tube sheets, flanges, forged tubes, shell courses | Listed in EN 10028-7 and AD 2000 W 2 |
| Heat exchangers | Tube sheets, channel covers, baffle rings | Chloride pitting resistance at PREN about 32 |
| Marine and chemical tankers | Flanges, valve bodies, pump shafts | Chloride cargo and seawater splash |
| Flue gas desulphurisation | Rings, discs, scrubber internals | Acidic chloride-bearing condensate |
| Valves | Stems, seat rings, bodies, blocks, plugs | Higher proof strength than 317L at same corrosion class |
| Cryogenic | Flanges, rings, structural forgings | Impact energy retained at minus 196 degrees C |
| Rotating equipment | Shafts, spindles, gears, rolls, crankshafts | Toughness plus corrosion resistance |

## 7. Availability

EN 10088-2 classes 1.4434 as an austenitic special grade. Availability guidance from
the British Stainless Steel Association rates it at level 4 for both flat and long
products, meaning it is normally obtainable only from mills when enough quantity is
ordered, not from a stockholder shelf. Because Jiangyin Jiangnan Metal Co., Ltd.
forges from ordered melt rather than standing stock, the grade can be supplied in
one-off and low-volume quantities and in sections no stockist carries.

## 8. Common questions

**What is X2CrNiMoN18-12-4?**
Material number 1.4434, a low-carbon nitrogen-alloyed austenitic stainless steel
defined in EN 10088-1 and EN 10088-2, with 16.5 to 19.5 percent chromium, 10.5 to
14.0 percent nickel, 3.0 to 4.0 percent molybdenum, 0.10 to 0.20 percent nitrogen and
carbon capped at 0.030 percent.

**Is it the same as 317LN?**
They are recognised equivalents: AISI 317LN, UNS S31753, JIS SUS 317LN, KS STS 317LN,
GB 022Cr19Ni13Mo4N. Where an order names ASTM A240 Type 317LN, the material must be
certified to that ASTM specification and not only to EN 10088.

**How does it compare with 316L?**
More molybdenum, 3.0 to 4.0 percent against roughly 2.0 to 3.0 percent, plus a
nitrogen addition 316L does not have. Result: higher chloride pitting and crevice
resistance, PREN around 32, and a higher minimum proof strength, which can allow a
thinner section at the same design pressure.

**What is the PREN?**
About 32, as a comparative index only.

**Can it be hardened by heat treatment?**
No. Strength is raised only by cold work. Supplied solution annealed, with published
practice for 317LN using 1080 to 1175 degrees C followed by rapid water quenching.

**Which ultrasonic testing standard applies?**
EN 10228-4 for austenitic stainless forgings. ASTM A388 or SEP 1921 on request.

**What sizes and shapes are available?**
All custom, to drawing. Seamless rolled rings, flanges, shafts, discs, bushings,
sleeves, tube sheets, bars, forged pipes and tubes, rolls and crankshafts. Send
dimensions, governing standard, required testing and certification level to
sales@steelforgepieces.com.

**What certification is provided?**
EN 10204 3.1, or 3.2 countersigned by a third party inspection body. Certificates
record melt route, chemical analysis, heat treatment condition, mechanical test
results and NDT results against the ordered standard.

## Related grades

A182 F44 (1.4547), 904L (1.4539), Sanicro 28 (1.4563), A182 F51 (2205),
A182 F53 (2507), A182 F55 (Zeron 100), Nitronic 50, A182 F321.

## Data sources

Composition limits per EN 10088-2. Minimum mechanical properties per EN 10028-7.
Cross-references per ISO 15510 and Stahlschluessel. Availability rating per the
British Stainless Steel Association. Typical physical and mechanical values describe
the grade and are not guaranteed. Published data does not replace the ordered
specification or the mill certificate for the heat supplied.

## Contact

Jiangyin Jiangnan Metal Co., Ltd., open-die forging factory
No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
+86 189-2135-9659 | sales@steelforgepieces.com | www.steelforgepieces.com